The research and development of crystal plane in cemented carbides is one of the hotspots in the field of cemented carbides both domestically and internationally. The microstructure of the alloy determines its mechanical properties; in WC-Co cemented carbides, the grain size and distribution of the WC phase, as well as the substructure within the grains, are important factors affecting the material’s mechanical properties [10-13]. WC grains have a close-packed hexagonal structure (crystal system P-6m2, a=0.2906nm, c=0.2837nm)24, and the habit planes of WC grains are two basal planes and three prismatic planes. WC grains are prismatic in three-dimensional space, with the basal plane being parallel to the (0001) crystal plane and the prism plane being parallel to the (1-100) crystal plane 5. On the basis of this basic shape, some of the edges and corners are replaced by new crystal planes?6-21. Given that cemented carbides with specific orientations can produce excellent mechanical properties to meet special application requirements, we believe that it is necessary to conduct in-depth research.

This paper takes WC-12Co cemented carbide as the research object. Firstly, nano WC-Co composite powders were prepared by in-situ reduction carbonization reaction at different temperatures, and the composite powders were rapidly densified by discharge plasma sintering technology. The sintered blocks were systematically studied to analyze the effect of the in-situ reduction carbonization reaction temperature on the distribution characteristics of special crystal planes.

Experiment

The raw materials used in the experiment were carbon black, blue tungsten (purity 99.5wt.%, average particle size 50μm) and cobalt oxide (purity 98.5wt.%, average particle size 35μm). Carbon black, blue tungsten, and cobalt oxide were weighed according to the proportion for generating WC-12Co powder, and high-energy ball milling was carried out in a hard alloy ball mill jar with ethanol as the ball milling medium. The mixed powders were subjected to in-situ reduction carbonization reaction at 850°C, 900°C, and 1000°C in a vacuum environment, with a holding time of 1 hour. 2wt% of grain growth inhibitor was added to the composite powders prepared by in-situ reaction, and discharge plasma sintering densification was carried out. The sintering temperature was 1080°C, the holding time was 5 minutes, and the sintering pressure was 60MPa.

材料 phase analysis was carried out on a Rigaku D/max-3c X-ray diffractometer with an acceleration voltage of 35kV and a current of 30mA, and a scanning rate of 2°/min. The micro-morphology of the powder was observed on a FEI-NovaNano SEM field emission scanning electron microscope.

Results and of Crystal Plane Distribution

Figure 1 shows the thermogravimetric (TG-DSC) curves of the nano WC-Co composite powder synthesized by in-situ reaction when heated to 1000°C at a heating rate of 10°C/min under Ar gas protection. From the change in the TG curve, it can be seen that as the temperature increases, the mass of the in-situ synthesized WC-Co composite powder decreases. When the temperature reaches 1000°C, the reaction ends, and the powder weight loss reaches nearly 6%. Throughout the heating process, the mass loss of the composite powder is divided into two stages: the first stage is from room temperature to 190°C, where there is a significant decrease in powder mass due to the ease of gas adsorption by nanoscale powders, and the gas desorbs and releases during the heating process, causing powder weight loss; the second stage is from 628°C to 1000°C, where the weight loss rate decreases from high to low. This is because the composite powder did not fully react during the low-temperature in-situ reduction carbonization reaction, and a secondary reaction occurred during the heating process, resulting in rapid weight loss of the powder.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 2

Figure 2 shows the nanoscale WC-Co composite powder prepared by in-situ reduction carbonization reaction at 850°C. The powder particle size is mainly distributed between 30~120nm, with an average particle size of ~83.4nm. The particles have a good sphericity, and spherical or quasi-spherical powders exhibit good dispersibility and flowability, which can effectively avoid hard agglomeration of the powder. This is beneficial for the uniform dispersion of the powder in the sintering mold, thereby ensuring the uniformity and density of the sintered bulk structure. The composite powder prepared by the in-situ reduction carbonization reaction is subjected to rapid sintering densification in an SPS system to obtain nearly fully dense WC-Co cemented carbide blocks. XRD tests are conducted on the alloy specimens in the direction perpendicular to the sintering pressure and in the direction parallel to the sintering pressure. The relative integral intensities (i.e., integral area) of the diffraction peaks for each crystal plane in the VD (vertical to the sintering pressure) and PD (parallel to the sintering pressure) planes of the specimens are obtained through fitting calculations and compared with the relative intensities (integral area) of the diffraction peaks for each crystal plane in the PDF card (which represents the diffraction peak intensity distribution characteristics of traditional sintered cemented carbides), as shown in Table 1. The results indicate that the sintered WC-Co cemented carbide block specimens exhibit a significant characteristic of high anisotropic distribution for specific crystal planes.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 3

Figure 3 shows the XRD patterns of the VD (vertical to the sintering pressure) and PD (parallel to the sintering pressure) planes of the specimens obtained by SPS sintering of the nanoscale WC-Co composite powder prepared by in-situ reaction at 850°C. From the figure, it can be observed that on the PD plane, the intensity of the (0001) plane peak is lower, while the intensity of the (10-10) plane peak is relatively higher. By fitting and calculating the integral area of each diffraction peak, the relative integral area of each crystal plane and the proportion of each crystal plane’s integral area in the total integral area are obtained, as shown in Figures 5 and 6.

 crystal plane distribution
crystal plane distribution

From Figure 5, it can be seen that on the PD plane, the integral area of the (0001) plane accounts for only 10.72% of the total integral area, which is a decrease of 3.3% from the 14.02% in the PDF card (as shown in Figure 4). The proportion of the (10-10) plane reaches 35.73%, which is higher than the 31.87% in the PDF card, and the proportion of the (10-11) plane decreases to 21.76% compared to the 28.11% in the PDF card. Compared to conventional cemented carbide samples, in the PD direction of the composite powder sintered block prepared by in-situ reaction at 850°C, the distribution proportion of the main characteristic planes (0001) and (10-11) decreases, while the distribution proportion of (10-10) increases.

 

Discussion

On the VD direction of the sample, as shown in Figure 6, the proportion of the (0001) crystal plane has significantly increased to 40%, compared to the 14.02% in the PDF card, while the proportion of the (10-10) crystal plane has decreased to 11.68%, a reduction of 20.19% from the 31.87% in the PDF card. From the above analysis, it can be understood that in the sintered block of composite powder prepared by in-situ reaction at 850°C, there is an orientation distribution of characteristic crystal planes. In the direction perpendicular to the pressure, WC grains rotate, causing the (0001) plane to become perpendicular to the pressure direction, thereby reducing the interfacial energy between WC grains. The sintered block of low-temperature in-situ reaction synthesis powder exhibits an orientation distribution characteristic of WC grain characteristic crystal planes, which is believed to be due to the formation of WC grains through secondary reactions during sintering, with atoms preferentially aligning along the (0001) plane and the rotation of WC grains under sintering pressure causing the (0001) plane to tend towards being perpendicular to the pressure direction.

When the temperature is raised to 900°C for in-situ reaction, the prepared composite powder is mainly WC with only a small amount of carbon-deficient phase. When the temperature is raised to 1000°C for in-situ reaction, pure WC-Co composite powder can be obtained. Since the crystal plane distribution of the grains in the powder is isotropic, the crystal plane distribution of WC grains does not change during the subsequent sintering densification process at 900°C and 1000°C, and they still exhibit a randomly distributed isotropic characteristic.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 4

結(jié)論

1) The nanoscale WC-Co composite powder prepared by low-temperature in-situ reduction carbonization reaction at 850°C can be sintered into cemented carbide block materials with a highly oriented distribution characteristic of WC grain crystal planes using SPS. The sintered blocks of in-situ reaction powder at 900°C and 1000°C maintain an isotropic distribution of WC grain characteristic crystal planes.

2) In the WC-Co cemented carbide with highly oriented characteristic crystal planes, the basal plane (0001) occupies the largest area fraction in the direction perpendicular to the sintering pressure, reaching 40.0%; the prism plane (10-10) occupies the largest area fraction in the direction parallel to the pressure, reaching 35.7%.

3) The phase purity of the composite powder generated by the in-situ reaction plays an important role in the crystal plane orientation of the sintered block. When the main phase of the composite powder is WC, the crystal plane distribution of the sintered block does not exhibit oriented characteristics. However, when the main phase of the composite powder is the carbon-deficient phase, the crystal plane of the sintered block presents an oriented distribution characteristic.

發(fā)表評(píng)論

電子郵件地址不會(huì)被公開。 必填項(xiàng)已用*標(biāo)注

欧美福利在线观看视频-日本少妇一区二区三区四区-日韩人妻丝袜中文字幕-亚洲一区二区三区最新视频| 国产成人综合激情婷婷-亚洲国产综合在线观看不卡-色综网久久天天综合狼人-亚洲av高清在线不卡| 亚洲欧美日韩另类第一页-亚洲欧美日本综合久久-亚洲一本之道高清在线观看-不卡在线一区二区三区视频| 在线观看91精品国产性-国产中文字幕精品免费-免费日韩毛片在线观看-精品人妻暴躁一区二区三区| 亚洲乱码中文字幕综合-欧美日韩亚洲综合久久精品-美女隐私无遮挡免费网站-国产精品激情av在线播放| 中文字幕乱码亚洲精品-亚洲伊人久久大香线蕉-麻豆视传媒视频短免费网站-极品美女被后入干出水视频| 亚洲国产成人精品毛片九色-成年片黄色大片品赏网-亚洲男人天堂色噜噜av-人妻免费精品久久一区| 日本大黄高清不卡视频在线-亚洲色图视频在线观看免费-国内精品自拍视频在线观看-av免费在线观看看看| 成年人有性生活正常吗-亚洲熟女熟妇五十路熟女熟妇-亚洲精品一区二区高清在线-日本视频在线播放91| 日韩欧美国产亚洲中文-亚洲国产av第一福利网-亚洲欧洲日韩一区二区三区-91精品国产福利线观看久久| 国产精品爽爽va在线观看-亚洲av永久一区二区三区综合-成人av免费大片黄在线观看-一本一道久久a久久综合精品| 国产精品羞羞答答色哟哟-最新麻豆精品在线视频-丰满多毛熟妇的大阴户-精品国产乱子伦一区二区三女| 午夜av毛片在线观看-青草精品视频在线观看-亚洲av中文字字幕乱码综合-午夜av一区二区三区中文字幕| 国产在线一区二区三区视频-国产一区二区三区成人18禁-国产精品自偷一区在线观看-熟女人妻片濑仁美在线| 国产精品大片中文字幕-国产丝袜av一区二区免费-亚洲av巨作一级精品-国产成人综合亚洲欧美天堂| 欧美日韩国产在线三级-少妇人妻精品一区二区三-调教熟妇女同在线观看中文字幕-亚洲成av人片一区二区三区不卡| 激情视频在线观看国产一区-日韩高清在线视频一区免费观看-国产白丝精品在线观看-色偷偷伊人大杳蕉综合网| 国产黑色丝袜在线观看网站-成人a免费大片在线看-熟妇人妻精品一区二区三区视频-日韩av高清不卡一区二区三区| 精品国产精品久久一区免费式-男女高清无遮挡免费视频-av男人的天堂一区二区三区-免费观看视频网站97| 国产亚洲欧美日韩俺去啦-91香蕉国产极品在线播放-国产夫妻生活自拍视频-永久免费的成年视频网| 黄色大片一级在线观看-蜜臀91精品国产高清在线-色综合久久鬼色综合久久-九九热精品视频在线免费看| 精品国产美女av天堂-狼人av在线免费观看-日韩精品人妻中文字幕有码在线-欧美视频亚洲视频自拍偷拍| 精品人妻中文字幕有码在线-亚洲欧美一区二区成人精品久久久-亚洲第一人伊狼人久久-亚洲国产欧美精品在线观看| 中文字幕亚洲天堂第一页-国产午夜福利在线视频-亚洲精品中文字幕女同-亚日韩精品一区二区三区| 国产精品国产一区日韩一区-老色99久久九九爱精品-国产亚洲精品福利一区-亚洲av乱码av一区二区三区| 人妻体内射精一区二区三区小视频-国产精品久久久久人人爽-日韩三级黄色一区二区三区-亚洲伊人色综合网收藏| 不卡一区二区三区视频-国产亚洲91精品色在线观看-国产精品青草久久福利不卡-国产黄色免费精品网站| 国产在线精品一区二区中文-亚洲小说欧美另类激情-97碰久日韩视频在线观看-日本一道本高清不卡区| 日韩有码中文在线视频-少妇我被躁爽到高潮在线观看-精品丰满人妻一区二区三区-亚洲天堂高清在线播放| 国产激情久久久久成熟影院-成人午夜免费在线视频-亚洲中文字幕成人综合网-色噜噜精品视频在线观看| 91福利精品第一导航-国产一区二区三区不卡精品-偷拍日本美女公厕尿尿-国产黄三级三级三级看三级| 日本一区二区三区四区黄色-91在线国产经典观看精品-亚洲一区二区三区免费不卡-av免费在线观看蜜臀| 国产精彩自拍视频在线-岛国视频免费在线播放-91久久精品国产综合另类专区-午夜福利欧美激情福利| 国产精品精品久久99-久久羞羞色院精品全部免费-日韩中文粉嫩一区二区三区-外国黄色三级视频网站| 久久99国产精品久久99蜜桃-国产在线精品福利91啪-日本啪啪免费观看视频-免费看的日麻批网站视频| 日韩黄色精品中文视频-久久精品国产亚洲懂色-欧洲美女日韩精品视频-国产一区二区三区精品愉拍| 国产精品蜜桃久久一区二区-久久精品熟女亚洲av麻豆蜜臀-日本一区二区精品色超碰-伊人一区二区三区久久精品| 亚洲av成人午夜福利在线观看-日韩精品成人影院久久久-国产在线高清不卡一区-激情五月另类综合视频| 亚洲熟女少妇av麻豆-男人一天堂精品国产乱码-欧美精品高清在线播放-亚洲国产午夜福利精品| 国产精品中文字幕在线一区-国产成人美女精品自在拍av-密桃av一区二区三区四区-女优免费中文字幕在线| 国产一区二区三区在线播放-偷拍女厕尿尿在线免费看-午夜一区二区三区三区-国产精品一区二区三上人妻|