Mining pick is one of the vulnerable parts in coal mining and roadway driving machinery, and it is the main tool for coal falling and coal breaking. Its performance directly affects the production capacity of coal mining machinery, power consumption, working stability and the service life of other related parts. With the increase of people’s demand for energy, especially for coal, in order to improve the mining efficiency, the power of the shearer is increasing, and the quality of the pick is required to be higher and higher. As the material of the shearer pick, it is required to have higher strength, hardness and wear resistance, bending strength and corrosion resistance.

Working process of shearer pick

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 2

Under the action of the front edge of the pick, the coal is broken and the large block is peeled off at the same time. At the moment when the tip contacts the coal, there are elastic and plastic deformation in the contact range of the tip. With the increase of the contact stress, when the strength limit is exceeded, the core is crushed into very fine powder to form a dense core, which is composed of the crushed coal under pressure. With the advance of the cutting tool, the dense core gradually grows and accumulates energy, and the cutting resistance also increases. The dense core compresses the front coal area and makes this part produce elastic deformation. Because the ore body around the dense core forms the stress state area, it actually plays a role in changing the geometry of the pick cutter head. When the contact stress of the cutter tip increases to the limit value, the dust in the area before the dense core ejects at a high speed, driving the small pieces to peel off.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 3

Failure form

The main failure forms are the invalidation of alloy cutter head, chipping of cutter head, wear of alloy cutter head and gear body. In some working conditions, the failure of pick is often caused by the fracture of gear body. As the mechanical performance of the pick body directly affects the service life of the pick, it is of positive significance to select the material and effective heat treatment method of the pick body reasonably to reduce the wear and fracture of the pick, reduce the consumption of the pick of the shearer, improve the operation rate of the shearer and increase the comprehensive economic benefits of the production of the shearer.

Wear and fracture failure

In the process of cutting coal seam, the pick has strong friction and abrasive wear with the coal seam. The most stressed point of the pick is at the head of the working part of the pick, where the wear is the most serious, resulting in the wear and failure of the pick pants. In the actual coal production, about 50% of the pick failure is caused by wear.

Breaking and invalidation of cemented carbide tooth head

The invalidation of cemented carbide is related to the hardness of ore in coal and rock: when the pick cuts coal and rock, if the hard ore in coal and rock is encountered, the cutter head is in the state of high-pressure stress, and it will bear high shear stress at the place where the contact between the cutting edge and coal and rock is poor, and it is in the state of tensile stress. When the tensile stress exceeds the strength limit of the alloy, the cutter head will break.

related to the poor brazing quality of tooth head.

For example, there are sand inclusions and microcracks in the weld, which cause the shear strength of the weld to be low. The abscission of cemented carbide is also related to the unreasonable size of weld gap. The use of less solder during brazing results in the loosening of cemented carbide head and the abscission of tooth head.

related to the low hardness and poor wear resistance of the working part

From the point of view of the material of the pick pant body, the reason for the invalidation of the carbide cutter head is related to the low hardness and poor wear resistance of the working part of the pick magazine body. The excessive wear of the part of the pick supporting the carbide results in the insufficient supporting force and the invalidation of the carbide. Therefore, by improving the hardness of the working part of the pick and the quality of brazing, the invalidation of cemented carbide can be avoided.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 4

Performance improvement method

1. According to the hardness index of coal and rock, the corresponding grade of alloy cutter head is selected. Generally, the compressive strength of coal or coal rock roadway can be selected with less Co. the compressive strength of roadway surrounding rock should adopt the use of advanced technology such as limited or manufacturing composite alloy material spraying to improve the impact resistance.

2. The manufacturing process shall be in strict accordance with the design requirements, to ensure the matching between the pick and the gear holder, to ensure that the tool can rotate freely in the gear holder, to avoid the phenomenon of eccentric wear, the automatic grinding function, to maintain the normal wear of sharp blade and even cutting teeth, in the cut state. Brazing and heat treatment process. Brazing and heat treatment process is one of the key technologies for cutting quality of pick.

3. A layer of niobium carbide hard alloy is deposited on the surface of the coal pick steel machine by using the hardfacing technology to obtain the hardfacing wear-resistant layer with metallurgical structure with the base. Niobium carbide is distributed on the iron-based martensite and retained austenite intensively in the trading net of Chinese shearer, which protects the collective from wear. The Hardmetals with high hardness in the hardfacing layer and a large number of metallographic structures that play the role of wear-resistant framework make the hardfacing layer have high wear-resistance.

4. Thermal spraying can heat a linear or powdery material to a melting or semi melting state and accelerate the formation of high-speed droplet by means of heat sources such as flame, arc or plasma, spray to the substrate to form a coating on it, which can strengthen the surface of the material and improve its wear-resistant and corrosion-resistant properties.

5. Plasma cladding is a new material surface modification technology which uses plasma beam as heat source to obtain excellent wear resistance, corrosion resistance, heat resistance, impact resistance and other properties of metal surface. Plasma cladding is a rapid non-equilibrium solidification process, which has many strengthening effects such as supersaturated solution strengthening, dispersion strengthening and precipitation strengthening.

6. The brazing and heat treatment process of the pick is one of the key technologies to ensure the quality of the pick. At present, the brazing and heat treatment of pick are integrated technology. It is heated by vacuum furnace, so that the brazed pick can be directly quenched without air cooling, and the brazing and heat treatment can be completed once. It can avoid the oxidation phenomenon of the traditional brazing surface contacting with the air, ensure the direct contact between the melted solder and the brazing surface, and ensure the welding quality; at the same time, because the brazing and heat treatment are completed once, it can avoid the embrittlement of the alloy head and the reduction of the weld strength caused by the two heating.

在线播放口爆吞精美女-亚洲精品中文字幕日韩在线-亚洲福利视频免费在线观看-精品国产自拍免费视频| 熟妇久久人妻中文字幕-国产精品久久久久精品三级人-亚洲蜜臀人妻中文字幕-国产一区二区内部视频| 日本亚洲一线二线三线-九月丁香婷婷啪啪色综合-狠狠综合欧美综合欧美色-亚洲丁香视频中文在线| 国产很黄免费观看久久-亚洲变态另类一区二区三区-欧美在线免费观看黄片-成人av不卡在线播放| 亚洲av免费网址大全-中文字幕日韩精品东京热-国产综合亚洲成人av-国产白丝美女av在线| 亚洲天堂男人的天堂在线-亚洲激情欧美日韩在线-国产av剧情精品老熟女-色老头与人妻中文字幕视频| 亚洲欧美成人影院网址-在线观看视频一区二区三区三州-成人自拍视频免费在线-国产精品蜜臀视频视频| 女生下面粉嫩在线视频-人妻熟女av国产在线-亚洲精品成人一区二区三区-商场偷拍女厕所撒尿视频| 极品国产粉嫩18尤物在线播放-中文字幕av人妻在线-国产一区二区三区乱码在线-最新亚洲av日韩av| 日本高清成人一区二区三区-亚洲国产精品久久成人-91福利国产午夜亚洲精品-极品激情国产剧情av| 四虎在线精品视频免费播放-日韩女同av在线观看-av日韩黄片在线播放-日本人体午夜福利视频| 国产视色精品亚洲一区二区-激情艺术中心国产精品-国产农村一级特黄真人片-免费观看午夜视频在线| 久久中文字幕亚洲天堂-午夜国产成人福利视频-亚欧天堂成人av成人-熟女乱中文字幕熟女熟妇| 五月婷婷六月色激情综合-国语对白在线免费视频-亚洲熟女熟妇乱色一区-深夜福利免费在线播放| 国产精品一区二区白浆视频-网红厕所天天干夜夜操a-日韩殴美精品一区二区-国产成人一区二区三区精品| 亚洲日本国产一区二区三区-日日噜噜夜夜狠狠免费-亚洲不卡在线视频观看-亚洲成年网站青青草原| 日韩成人大片一区二区三区-国产一级淫片av免费-18禁免费观看网站入口-国产黄色特级片一区二区三区| 蜜桃视频大全免费观看-国产高清不卡一区二区-亚洲av综合av东京热三区-无套内射激情国产av| 一本久道视频无线视频试看-亚洲国产精品一区二区三区久久-中文字幕色偷偷人妻久久-久久精品99国产精品中| a在线观看视频在线播放-81精品人妻一区二区三区蜜桃-国产午夜福利片一级做-在线观看亚洲视频一区二区| 亚洲国产日韩精品欧美银杏-99久久免费热在线精品-国产精品免费不卡av-国产精品老熟女视频一区二区| 国产欧美日韩一区二区三区88-国产亚洲av嫩草精品影院-成人国产一区二区三区麻豆-在线观看午夜宅男视频| 美女脱内衣内裤露出咪咪-美女一区二区三区免费观看-国产网红女主播在线视频-久久亚洲春色中文字幕| 亚洲欧美日韩另类影院-亚洲一区二区三区精品春色-精品人妻久久一品二品三品-人妻有码av中文字幕久久午夜| 爆操美女屁股在线观看免费-亚洲国产成人久久综合-亚洲一区二区免费中文麻豆-青青青青草原在线观看| 视频一区二区不中文字幕-亚洲av色香蕉一区二区三区妖精-国产91精品在线观看懂色-国产一区二区三区不卡在线看| 国产精品成久久久久久三级四虎-亚洲成人av在线高清-国产精品一区二区三区自拍-欧美午夜激情视频网站| 精品国产成人亚洲午夜福利-午夜福利一区二区91-亚洲中文字幕女优最新网址-亚洲av成人国产精品| 久热99在线视频免费观看-黄片视频在线免费观看国产-国产精品av国产精华液-av在线男人的免费天堂| 亚洲av成人精品爽爽-国产麻豆91在线播放-国产精品久久精品久久精品-蜜臀久久综合一本av| 尤物国产精品福利在线网-中日韩一二三级黄色永久视频-加勒比av免费在线播放-91欧美精品一区二区三区| 亚欧曰中文字幕av一区二区三区-最新国产情侣在线视频-黄片大全视频免费在线观看-久久超级碰碰碰一区二区三区| 国语对白高清在线观看-久久av精品一区二区三区-日韩在线中文字幕不卡-免费视频成人高清观看在线播放| 久久噜噜噜精品国产亚洲综合-91精品国产高清久久福利-精品国产一区二区三区麻豆-日本加勒比一区二区在线观看免费| 日韩成人av在线影院-亚洲五月天久操视频在线观看-最新国产AV无码专区亚洲-欧美日韩大香蕉在线视频| 美女被狂躁到高潮视频-国产熟女精品自拍视频-亚洲中文字幕在线精品一区-成人在线中文字幕电影| 国产一区二区三区视频网站-日韩av影片免费在线观看-日韩av有码免费在线观看-制服丝袜天堂网在线观看| 追虎擒龙国语高清在线观看完整版-色婷婷一区二区三区免费-网友自拍在线视频国产-草草久在线视频在线观看| 精品人妻一区二区三区三区四区-亚洲中文字幕熟女一区二区-91久久精品国产91性色69-国产精品中文字幕中文字幕| 久99久热这里只有精品-日韩av一区二区三区播放-天堂日韩av在线播放-中文字幕被侵犯的人妻| 激情综合网激情国产av-2021日韩午夜影院-精品一区二区三区少妇蜜臀-人妻交换av一区二区|