色呦呦网址在线观看,久久久久久久久福利精品,国产欧美1区2区3区,国产日韩av一区二区在线

Shield tunneling cutter are the key supporting tools for tunneling?machines, and their performance and service life determine the excavation efficiency of the entire project.

carbide?shield tunneling cutter?usually come in three types:

1Soft soil cutter: used for excavation in soft soil, sand layers, and small particle sandstone formations where the stratum is loose and there is no need to break the rock layer with a roller cutter. The scraper is used to scrape and disturb the face only, and all tools are carbide cutting blades.

2Composite cutte : used for excavation in various geological formations such as sand and rock layers. In this case, the rock needs to be broken by the roller cutter, and then the scraper is used to scrape off the part of the rock between the two cutter rings. As the rock has already been compressed and cracked by the roller cutter, it is no longer dense, and the scraper can easily cut it. Therefore, the tools in this case are composed of roller cutters and carbide cutting blades.

3 Hard rock cutter: used for excavation in highly dense pure rock formations. The roller cutter breaks the rock, and as the cutter continues to penetrate, the cracks connect and form slag, which is peeled off from the surface of the cutter head. There is no need for a carbide scraper to scrape the residual rock, so no carbide tools are required. Only several wear-resistant steel plates need to be set at the slag discharge port to collect the slag. Therefore, the tools in this case consist of roller cutters and wear-resistant scraper blades.

The 2 Typical Failures of Carbide Shield Tunneling Cutter and How do We Tackle Them 1

Forms of failure for carbide?shield tunneling?cutters

Through a large number of engineering practices, it has been found that the proportion of tool failure caused by normal wear to the limit is only about 45% of all failed tools. The proportion of carbide cracking in the failure of carbide shield tunneling cutters is about 35%, the proportion of carbide shedding in all cutter damage is about 15%, and the proportion of tool failure caused by other reasons is only about 5%.

The following are several common forms of failure for carbide?cutters:

 

carbide?cracking

Cracking refers to the phenomenon of carbide?fracturing under external impact force. The reasons for the cracking of the shield tunneling cutter?are as follows:

1 Improper selection of carbide?grade. If high wear-resistant and low toughness carbide?is selected in high-impact formations, it is extremely easy to cause carbide?cracking.

2 Problems with welding process. carbide?and steel substrate are brazed with copper-based/silver-based solders. Improper control of the welding process will cause microcracks in the carbide, and subsequent impact will cause crack propagation, ultimately leading to alloy cracking.

3 Poor welding heat treatment.

a.If the carbide is not heated to a certain temperature before welding and directly heated by medium-frequency induction, the welding process will generate excessive thermal stress.

b.If the welded cutteris not immediately quenched in a tempering furnace after welding, the alloy and steel substrate will cool too quickly, and the difference in thermal expansion coefficients between the carbideand steel will cause inconsistent shrinkage during the cooling process, leading to carbide being pulled apart.

c.Improper shield operation when encountering geological mutations or isolated rocks. If the shield encounters geological mutations, uneven hardness of the formation, or isolated rocks during operation, and the shield driver does not notice or take measures, the cutterwill be subjected to a huge impact, causing carbide to crack.

 

Carbide detachment

carbide?detachment refers to the phenomenon where the carbide?completely separates from the steel substrate. The main reasons for carbide?detachment are as follows:

Poor brazing process between carbide?and steel substrate, resulting in insufficient bonding strength. When cutting through rock and soil, the welding seam between the carbide?and steel is pulled apart, causing the alloy to detach. The industry-recognized bonding strength for carbide?and steel brazing is 245 MPa. Only by improving the brazing strength can the carbide?be prevented from easily detaching.

shield tunneling cutters

To make a conclusion, common forms of shield cutter failure include three types: cutter cracking, cutter deformation, and excessive wear. The main reason for cutter cracking is that the heat treatment hardness is too high or the hardness distribution is uneven. The main cause of cutter deformation is improper selection of cutter material or insufficient consideration of stress in the design. The main reason for excessive wear of the cutter body is improper selection of cutter material or insufficient wear-resistant cladding protection.

 

Ways to improve the lifespan of shiled tunneling cutters

Do a good carbide grade selection

For shield tunneling,due to the variability of geological conditions, a coarser WC particle size is required for the carbide. Therefore, commonly used grades are listed in order of increasing cobalt content: YG8C, YG11C, YG13C, and YG15C. In this order, the wear resistance of these carbides decreases while their impact toughness increases (see fig. 1).

The 2 Typical Failures of Carbide Shield Tunneling Cutter and How do We Tackle Them 2

fig.1

Get a reasonable material?selection of cutter substrate body

Q345 and Q235 are commonly used for cutter body materials in China. These two materials have low alloy elements and carbon content, making it impossible to significantly improve their material hardness and strength through heat treatment. As a result, the wear resistance and strength of the steel matrix are relatively low, and the probability of wear, deformation, and fracture is high. 40Cr, 42CrMo, 35CrMo, and 40CrNiMo alloy structural steel can be used as matrix materials, which contain various metal elements, improve the quenching ability of steel itself, and increase the hardness of the steel matrix to HRC 38-42 after heat treatment. Its impact resistance and fatigue strength are comprehensively improved.

 

carbide?brazing process?is important

Silver-based brazing is increasingly used in the welding of shiled tunneling cutter. It is known for its low temperature, good fluidity, and small welding stress, which greatly reduces the phenomenon of carbide virtual welding. Additionally, due to the low temperature, the welding process causes less damage to the carbide, and the possibility of forming welding stress and micro-cracks is smaller.

 

Wear-Resistant Overlaying Protection

In addition to carbide?and steel matrix, wear-resistant overlaying is also required for cutter tools. The main component of wear-resistant overlaying is tungsten-cobalt, which is remelted on the surface of the steel matrix by arc or plasma welding. This protects the cutter tool from wear and extends its service life.

 

Design?principle?of shield tunneling cutter matters

Cutter performance is not only related to the manufacturing process but also closely linked to the tool design. If the design is excellent, the performance of each part of the cutting tool can be utilized to its fullest potential. The tool may encounter a problem where the steel billet was bent and fractured. This problem was solved by changing the structure, which eliminated the issues of tool fracture and bending.

 

Reduce tunneling advancement methods’ impact

1 Attention should be paid to controlling the excavation parameters during shield tunneling. For example, when there is a geological mutation, the speed of the cutterhead and the advancement of the shield should be cut to reduce the impact of the geological mutation on the tools and avoid tool damage.

2 During the tunneling process, foam should be added in a timely manner and slurry soil should be improved to enhance its performance and reduce wear. The temperature of the slurry soil should be monitored to prevent excessive temperature that can aggravate tool wear.

3 Strengthen tool management, regularly inspect and replace tools to prevent one tool from failing and causing increased loads on adjacent tools, thus accelerating their damage rate. After replacing the tool, a low thrust and low-speed test push should be conducted to give the tool a buffering time.

 

Conclusion

1 In order to improve the service life of cutting tools, it is difficult to achieve significant results by improving them in only one aspect. Only by improving cutting tools from multiple aspects such as design, manufacturing, and application can their performance be maximized.

2 After abnormal failure of cutting tools, starting from the mechanism of damage and finding the root cause of the failure can achieve good results by adopting targeted measures.

 

 

 

 

 

Leave a Reply

Your email address will not be published. Required fields are marked *

邻居少妇毛多水多太爽了-男人天堂手机在线视频-国产精品国产三级国产专播-韩国女主播福利视频一区二区| 亚洲高清无吗视频在线播放-国产亚洲最新在线不卡-久久亚洲国产精品成人-二区三区在线免费观看视频| 亚洲精品成人久久av中文字幕-中文av毛片在线观看-一本之道加勒比在线视频-日韩av一区二区在线观看不卡| 正在播放后入极品美少妇-亚洲一区二区三区自拍麻豆-国产亚洲精品成人久久-av老司机亚洲精品久久| 国产精品熟女露脸对白-欲求不满中文字幕在线-日本一区二区三区的免费视频观看-激情久久av一区二区三区四区| 成人一区二区三区激情视频-久久一区二区免费蜜桃-钢琴考级三级咏叹调视频-亚洲性感毛片在线视频| 亚洲一区二区三区视频观看-日韩精品一二三四区视频-亚洲码与欧洲码区别入口-日韩精品大片一区二区三区| 亚洲天堂成人av影院-日韩精品国产一区在线久草-欧美国产另类久久久精品-91午夜精品久久香蕉| 能看免费欧美一级黄片-男女视频网站免费精品播放-日本高清在线一区二区三区-熟女少妇免费视频网站观看| 国产一级亚洲一级一区-国产精品一亚洲av日韩av-日韩高清有码中文字幕-久久国产精品免费一区二区三区| 日韩三级在线视频不卡-国内自拍色第一页第二页-96热久久这里只有精品-日韩精品有码一区二区三区久久久| 国产老熟女精品一区二区三区-精品国精品自拍自在线-亚洲国内自拍愉拍少妇-欧美日韩一级片免费播放| 开心五月激情综合久久爱-国产精品深夜在线观看-91亚洲国产成人精品一区.-精品亚洲国产成人性色av| 久久久精品国产亚洲av高清涩受-国产精品一区二区三区成人-欧美日韩国产精品视频一区二区三区-大陆美女阴户特写毛片| 久久精品蜜桃一区二区三区-久久99亚洲精品久久-激情文化变态另类快播-国产成人免费永久在线平台| 日韩人妻毛片中文字幕-国产精品亚洲综合第一页-国产精品久久亚洲av-亚洲国产精品一区二区不卡| 亚洲av无一区二区三区久久-色琪琪久久综合网天天-国产一区二区视频在线播放-大象焦伊人久久综合网| 久久精品一区二区三区激情-男人天堂手机成人在线-激情五月色婷婷中文字幕-国产精品久久久久久人四虎| 国产大波精品一区二区在线-男女床上激情免费网站-日韩成人在线高清视频-国产精品视频免费自拍| 国产在线观看av自拍-成人自拍小视频在线看-十八禁网站在线免费观看-丰满的熟妇露脸大屁股| 国产偷拍自拍视频在线观看-丰满欧美熟妇视频在线-亚洲午夜激情在线观看-四虎视频精品免费观看| 人妻少妇中文字幕久久精品-水蜜桃av一区二区三区在线观看-日韩熟女精品一区二区三区-久久国产综合激情对白| 亚洲av成人精品爽爽-国产麻豆91在线播放-国产精品久久精品久久精品-蜜臀久久综合一本av| 国产精品性色av免费-人妻系列中文字幕一区二区-精品一区二区三区在线日韩-亚洲欧美日韩国产一二三区| 免费人成视频在线播放-成人级a爱看片免费观看-激情偷乱在线视频播放网-激情综合网激情综合网激情| 一区二区三区岛国av毛片-国产男女无遮挡猛进猛-久久精品人妻丝袜乱一区二区三区-国产超级对对碰在线观看| 尤物视频在线观看网址-欧美午夜精品久久福利-久久这里只有精品视频5-国产精品成人综合色区| 3p人妻一区二区三区-亚洲精品国产高清自拍-女同国产日韩精品在线-亚洲午夜国产激情福利网站| 日韩有码中文字幕在线视频-草草影院国产在线观看-日韩中文字幕有码午夜美女-亚洲第二十页中文字幕| 日韩精品中文一区二区三区在线-午夜视频国产在线观看-日韩中文字幕av有码-最新日韩精品视频免费在线观看| 亚洲综合不卡一区二区三区-中文字幕一区二区人妻秘书-国产免费午夜精品理论-中文字幕人妻精品一区二区| 97资源视频在线观看-青草视频在线免费播放-最新日韩中文字幕在线播放-成人国产av精品麻豆网站| 91高清在线观看播放-av在线免费观看男人天堂-九九热在线视频免费观看-美女脱内裤露出隐私部位| 亚洲视频第一页在线观看-最新中文字幕国产精品-中文人妻熟妇人伦精品熟妇-国产福利91在线视频| 国产精品免费av一区二区-91在线日本在线观看-免费在线激情视频网址-亚洲午夜福利影院在线免费观看| 日本厕所偷拍美女尿尿视频-婷婷国产一区综合久久精品-欧美一日韩成人在线视频-四虎精品视频免费在线观看| 97中文字幕一区二区三区-国产精品亚洲av无人-亚洲国产精品自产拍久久-成人深夜福利在线视频| 91福利精品第一导航-国产一区二区三区不卡精品-偷拍日本美女公厕尿尿-国产黄三级三级三级看三级| 成人国产精品一区二区香蕉-一区二区三区欧美日韩电影在线观看-午夜福利视频合集一区二区-人妻少妇被粗大爽在线| 一区二区三区四区五区黄色-色哟哟精品免费专区在线-很色精品99在线观看-亚洲一区二区三区精品久久| 麻豆国产av一区二区精品-久久福利社最新av高清精品-丝袜美腿亚洲综合伊人-亚洲欧洲av一区二区三区|