Mining pick is one of the vulnerable parts in coal mining and roadway driving machinery, and it is the main tool for coal falling and coal breaking. Its performance directly affects the production capacity of coal mining machinery, power consumption, working stability and the service life of other related parts. With the increase of people’s demand for energy, especially for coal, in order to improve the mining efficiency, the power of the shearer is increasing, and the quality of the pick is required to be higher and higher. As the material of the shearer pick, it is required to have higher strength, hardness and wear resistance, bending strength and corrosion resistance.

Working process of shearer pick

Знаете ли вы причину выхода из строя кирки и способ повышения ее производительности? 2

Under the action of the front edge of the pick, the coal is broken and the large block is peeled off at the same time. At the moment when the tip contacts the coal, there are elastic and plastic deformation in the contact range of the tip. With the increase of the contact stress, when the strength limit is exceeded, the core is crushed into very fine powder to form a dense core, which is composed of the crushed coal under pressure. With the advance of the cutting tool, the dense core gradually grows and accumulates energy, and the cutting resistance also increases. The dense core compresses the front coal area and makes this part produce elastic deformation. Because the ore body around the dense core forms the stress state area, it actually plays a role in changing the geometry of the pick cutter head. When the contact stress of the cutter tip increases to the limit value, the dust in the area before the dense core ejects at a high speed, driving the small pieces to peel off.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 3

Failure form

The main failure forms are the invalidation of alloy cutter head, chipping of cutter head, wear of alloy cutter head and gear body. In some working conditions, the failure of pick is often caused by the fracture of gear body. As the mechanical performance of the pick body directly affects the service life of the pick, it is of positive significance to select the material and effective heat treatment method of the pick body reasonably to reduce the wear and fracture of the pick, reduce the consumption of the pick of the shearer, improve the operation rate of the shearer and increase the comprehensive economic benefits of the production of the shearer.

Wear and fracture failure

In the process of cutting coal seam, the pick has strong friction and abrasive wear with the coal seam. The most stressed point of the pick is at the head of the working part of the pick, where the wear is the most serious, resulting in the wear and failure of the pick pants. In the actual coal production, about 50% of the pick failure is caused by wear.

Breaking and invalidation of cemented carbide tooth head

The invalidation of cemented carbide is related to the hardness of ore in coal and rock: when the pick cuts coal and rock, if the hard ore in coal and rock is encountered, the cutter head is in the state of high-pressure stress, and it will bear high shear stress at the place where the contact between the cutting edge and coal and rock is poor, and it is in the state of tensile stress. When the tensile stress exceeds the strength limit of the alloy, the cutter head will break.

related to the poor brazing quality of tooth head.

For example, there are sand inclusions and microcracks in the weld, which cause the shear strength of the weld to be low. The abscission of cemented carbide is also related to the unreasonable size of weld gap. The use of less solder during brazing results in the loosening of cemented carbide head and the abscission of tooth head.

related to the low hardness and poor wear resistance of the working part

From the point of view of the material of the pick pant body, the reason for the invalidation of the carbide cutter head is related to the low hardness and poor wear resistance of the working part of the pick magazine body. The excessive wear of the part of the pick supporting the carbide results in the insufficient supporting force and the invalidation of the carbide. Therefore, by improving the hardness of the working part of the pick and the quality of brazing, the invalidation of cemented carbide can be avoided.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 4

Performance improvement method

1. According to the hardness index of coal and rock, the corresponding grade of alloy cutter head is selected. Generally, the compressive strength of coal or coal rock roadway can be selected with less Co. the compressive strength of roadway surrounding rock should adopt the use of advanced technology such as limited or manufacturing composite alloy material spraying to improve the impact resistance.

2. The manufacturing process shall be in strict accordance with the design requirements, to ensure the matching between the pick and the gear holder, to ensure that the tool can rotate freely in the gear holder, to avoid the phenomenon of eccentric wear, the automatic grinding function, to maintain the normal wear of sharp blade and even cutting teeth, in the cut state. Brazing and heat treatment process. Brazing and heat treatment process is one of the key technologies for cutting quality of pick.

3. A layer of niobium carbide hard alloy is deposited on the surface of the coal pick steel machine by using the hardfacing technology to obtain the hardfacing wear-resistant layer with metallurgical structure with the base. Niobium carbide is distributed on the iron-based martensite and retained austenite intensively in the trading net of Chinese shearer, which protects the collective from wear. The Hardmetals with high hardness in the hardfacing layer and a large number of metallographic structures that play the role of wear-resistant framework make the hardfacing layer have high wear-resistance.

4. Thermal spraying can heat a linear or powdery material to a melting or semi melting state and accelerate the formation of high-speed droplet by means of heat sources such as flame, arc or plasma, spray to the substrate to form a coating on it, which can strengthen the surface of the material and improve its wear-resistant and corrosion-resistant properties.

5. Plasma cladding is a new material surface modification technology which uses plasma beam as heat source to obtain excellent wear resistance, corrosion resistance, heat resistance, impact resistance and other properties of metal surface. Plasma cladding is a rapid non-equilibrium solidification process, which has many strengthening effects such as supersaturated solution strengthening, dispersion strengthening and precipitation strengthening.

6. The brazing and heat treatment process of the pick is one of the key technologies to ensure the quality of the pick. At present, the brazing and heat treatment of pick are integrated technology. It is heated by vacuum furnace, so that the brazed pick can be directly quenched without air cooling, and the brazing and heat treatment can be completed once. It can avoid the oxidation phenomenon of the traditional brazing surface contacting with the air, ensure the direct contact between the melted solder and the brazing surface, and ensure the welding quality; at the same time, because the brazing and heat treatment are completed once, it can avoid the embrittlement of the alloy head and the reduction of the weld strength caused by the two heating.

乱中年女人伦中文字幕久久-国产成人高清免费视频网站-中文字幕亚洲人妻在线视频-中文字幕剧情av在线| 91高清在线观看播放-av在线免费观看男人天堂-九九热在线视频免费观看-美女脱内裤露出隐私部位| 日本人妻中文字幕有码视频-男女啪啪视频免费观看一区-青青草原综合在线视频-极品人妻少妇精品一区二区| 亚洲欧美日本成人在线-伦理视频在线观看一区二区三区-日韩精品中文字幕人妻-四虎永久地址在线观看| 国产精品一区成人精品果冻传媒-日韩精品一区二区三区不长视频-欧美日韩不卡在线视频-99久久热视频在线观看| 国产一级r片内射视频播放-中文字幕最新精品资源-久久青青草原精品国产麻豆综合-深夜成人在线免费视频| 亚洲中文字幕中出在线-美女口爆吞精在线播放-亚洲欧美清纯唯美另类-国产一区二区三区免费观看不卡| 午夜中文字幕一区二区三区-亚洲精品av在线免费观看-蜜臀av一区二区三区久久bu-五月激情综合在线视频| 加勒比中文字幕久久av-久久黄色美女三级久一点黄-国产精品无套高潮久久-久久婷婷综合色拍亚洲| 日本一区二区三区在线视频-国产午夜性生活免费视频-亚洲老熟妇av熟妇在线-久久热这里只有精品国产| 精品国产高清一区二区广区-午夜少妇激情视频网站-亚洲av日韩精品一区在线-青草亚洲免费在线观看| 丰满女性丰满女性性教视频-国产日韩欧美精品av-日韩区一区二区三区在线观看-四虎国产精品成人免费久久| 亚州国产精品一区二区-尤物在线观看视频免费-国产91久久精品视频-一色桃子中出欲求不满人妻| 国产午夜视频在线观看720p-成人深夜福利av在线-一区二区日韩精品教师学生-亚洲一区二区三区美臀在线播放| 国产亚洲成人精品久久久-亚洲免费av高清在线观看-在线观看国内自拍视频-亚洲国产成人精品综合色| 国产老熟女乱子一区二区-欧美日本中国一区二区-欧美日韩国产午夜精品-青青草视频在线观看入口| 亚洲一区日韩精品在线观看-精品人妻少妇一区二区免费蜜桃-国产三区四区五区在线观看-真正国产熟女免费视频| 少妇高潮真爽在线观看-韩国福利视频一区二区三区-警花av一区二区三区-尤物视频国产在线观看| 亚洲精品成人久久av中文字幕-中文av毛片在线观看-一本之道加勒比在线视频-日韩av一区二区在线观看不卡| 能看免费欧美一级黄片-男女视频网站免费精品播放-日本高清在线一区二区三区-熟女少妇免费视频网站观看| 综合久久少妇中文字幕-亚洲中文波霸中文字幕-免费在线看的av网站-久久狠狠爱亚洲综合影院| 一区二区三区日本在线播放-男人的天堂亚洲最新在线-各类女厕正面偷拍精品-91精品蜜臀国产自产| 不卡一区二区三区视频-国产亚洲91精品色在线观看-国产精品青草久久福利不卡-国产黄色免费精品网站| 婷婷激情五月天第四色-岛国片av在线免费观看-久久综合久久一区二区-91青青草原免费观看| 日本一区二区三区四区高清-91久久香蕉国产熟女-久久精品99国产日本精品-国产粉嫩一区二区三区在线观看| 亚洲国产日韩精品欧美银杏-99久久免费热在线精品-国产精品免费不卡av-国产精品老熟女视频一区二区| 激情六月综合激情六月-韩国国产日韩在线观看视频-久久精品国产亚洲av高清色-亚洲熟女乱码一区二区三区| 少妇一级aa一区二区三区片-欧美欧美欧美欧美一级片-91在线观看视频下载-自拍视频在线观看一区二区| 国产精品剧情一区在线观看-精品伊人久久大香线蕉-一起草视频在线播放观看-精品少妇人妻av一区二区蜜桃| 91精品在线播放黑丝后入-97免费在线播放视频-av网站天堂网国产av-亚洲熟妇乱色一区二区三区| 免费观看国产裸体视频-久久亚洲精精品中文字幕早川悠里-99精品国产一区二区青青牛奶-久久精品成人av免费观看| 2020天天操夜夜操-亚洲色图视频在线观看,-亚洲色图专区另类在线激情视频-岛国精品毛片在线观看| 国产成人午夜精品久久-91久久精品一区二区喷水喷白浆-中文字幕日本人妻99-美女人妻少妇一区二区三区| 中文字幕av东京热久久-国产精品日韩精品最新-亚洲激情av免费观看久久-亚洲第一精品国产网站| 尤物视频在线观看精品-日韩午夜男女爽爽影院-日本少妇下面好紧水多影片-国产亚洲精品视频在线网| 99久久久国产精品视频-亚洲最大的福利视频网站-日韩人妻精品一区二区在线-中文字幕乱码精品在线观看| 精品国产乱码一二三区在线-精品国产一区二区在线视-国内男女精品一区二区三区-亚洲中文字幕国内精品| 美性中文网美性综合网-亚洲最大黄色网在线观看-自偷精品视频三级自拍-97精品伊人久久大香| 日韩人妻毛片中文字幕-国产精品亚洲综合第一页-国产精品久久亚洲av-亚洲国产精品一区二区不卡| 中文字幕在线成人大片-日本一区二区在线视频播放-精品在线亚洲一区二区三区-在线免费观看播放视频| 亚洲高清日本一区二区三区-日韩极品精品一区二区三区-亚洲成人av在线一区二区-亚洲精品国产精品粉嫩|