Overview

In recent years, research on coarse grain carbide grades and materials has been advancing in two different directions: ultra-coarse and ultra-fine grains. Ultra-coarse grain cemented carbides have been widely applied in mining rock drilling tools, roll mills, and stamping molds.

Studies have revealed several primary forms of carbide failure during drilling: impact fatigue, abrasive wear, and thermal fatigue. For hard rock formations, such as granite (drilled with impact or rotary impact drills), abrasive wear is relatively lower, and carbide failure is primarily caused by impact and impact fatigue. The compressive strength and bending strength of the carbide are directly related to its impact fatigue resistance; additionally, this resistance is associated with the carbide’s purity, WC grain size, and Co phase’s average free path. Furthermore, the carbide’s impact fatigue resistance is directly related to the impact energy.

Reasons for Issues in Cemented Carbide Rock Drilling

For medium-hard rock formations, such as quartzite (drilled with impact drills), abrasive wear dominates. Abrasive wear generally consists of two aspects: micro-cracks at the contact points of abrasive particles and premature wear of the Co phase. The former primarily occurs on hard and brittle carbides, especially when abrasives have high fracture strength; the latter occurs on softer carbides with higher Co content, particularly when abrasives are very brittle. Figure 1 shows a scanning electron microscope (SEM) image of the wear surface of a GF20D grade drill tooth, produced by Xiamen Jinlu Special Carbide Co., Ltd., after drilling about 500 meters into quartzite. The YG6 grade carbide, composed of 94% WC with a grain size of 2-3 μm and 6% Co, has a hardness of HV30:1430. The image illustrates typical abrasive wear, characterized by premature Co phase wear and cracking and spalling of the WC phase.

For soft rock formations, such as sandstone, thermal fatigue is the primary cause of carbide failure, accompanied by abrasive wear. For ultra-soft rock formations, such as calcite and limestone, thermal fatigue is the main cause of carbide failure. The propagation of cracks and premature wear of the Co phase directly impact the drill tooth’s lifespan. Especially when drilling magnetite, thermal fatigue cracks, also known as creep cracks, dominate. Figure 2 shows a typical undulating cracking morphology of cemented carbide drill teeth formed while drilling magnetite. Figure 3 is an SEM image of a traditional polished cross-section of a carbide drill tooth that drilled about 5 meters into magnetite, composed of 94% WC with a grain size of 5 μm and 6% Co, with a hardness of 1230 HV. The image reveals that the thermal fatigue cracks on the carbide surface have extended into the carbide’s interior.

How Are New Grades of Ultra-Coarse Grain Rock Drilling Cemented Carbide Developed? 1

Figure 1: SEM photo of the wear surface of the quartzite at a depth of about 500 meters on the YG6 drill tips inserted in drill bits

 

How Are New Grades of Ultra-Coarse Grain Rock Drilling Cemented Carbide Developed? 2

Figure 2. Typical ups and downs of crack morphology formed when carbide drill teeth drill magnetite

 

How Are New Grades of Ultra-Coarse Grain Rock Drilling Cemented Carbide Developed? 3How Are New Grades of Ultra-Coarse Grain Rock Drilling Cemented Carbide Developed? 4

Figure 3. The carbide drill teeth drill a conventional polished cross-section of about 5m into the magnetite. The grade consists of 94% WC with a grain size of 5um and 6% Co with a hardness of 1230HV(SEM).

 

Reasons for Developing New Rock Drilling Cemented Carbides

The fundamental reason for developing new rock drilling carbides lies in the continuous advancement of mining and drilling technology both domestically and internationally. As drilling equipment becomes more advanced and drilling efficiency improves, there is a growing use of fully hydraulic, high-power, and high-efficiency rock drilling rigs and rotary-percussion drills. This advancement has raised higher demands for the quality and lifespan of rock drilling cemented carbides. When drilling tools penetrate rock, the pressure rises from 0 to 10 tons within 1/10 of a second, and the temperature increases from 20°C to 1000°C. During impact and rotation, drilling carbides generate extremely high temperatures. Especially when drilling magnetite, rapid formation of thermal cracks, commonly referred to as “snake skin” or “tortoise shell” cracks, occurs.

 

To meet the requirements of modern rock drilling technology, the performance of rock drilling cemented carbides needs to be improved and optimized in several key areas: the thermal conductivity (the ability of the material to conduct heat) should be as high as possible; the thermal expansion coefficient (the linear expansion of the material when heated) should be as low as possible to ensure minimal growth rate of thermal cracks; high-temperature hardness should be further enhanced to guarantee good wear resistance at high temperatures; in addition, the transverse rupture strength (TRS) and fracture toughness (Kic, the material’s ability to resist sudden fractures caused by micro-cracks) should also be improved.

 

Table 1 lists the thermal performance data of pure WC, pure Co, three commonly used WC-Co carbide grades, and three types of rock. These three grades, with varying Co content and WC grain sizes, are suitable for different rock drilling teeth, hot-rolled rolls, and multi-purpose applications.

How Are New Grades of Ultra-Coarse Grain Rock Drilling Cemented Carbide Developed? 5

Directions for Developing New Rock Drilling Cemented Carbides

It is well known that Co has low thermal conductivity and a high thermal expansion coefficient. Therefore, the Co content should be minimized as much as possible. On the other hand, cemented carbides with high Co content exhibit better strength and fracture toughness. From a mechanical perspective, especially when carbide drill bits penetrate rock surfaces at high speeds, the drill bits endure high impact and loads, or mechanical vibrations under hard cutting conditions, necessitating improved strength and fracture toughness in the carbide. Additionally, compared to fine-grained carbides, coarse WC grain sizes contribute to greater strength and fracture toughness of the cemented carbide.

As a result, the preparation of rock drilling cemented carbides tends to use lower cobalt content and increase WC grain size to achieve good mechanical properties and the required high-temperature wear resistance. This approach results in ultra-coarse grain carbides. Traditionally, the production of ultra-coarse grain cemented carbides involves high-temperature reduction of coarse grain tungsten powder followed by high-temperature carburization to produce coarse grain WC powder. This powder is then mixed with Co powder and ball-milled to form a mixture, which is subsequently pressed and sintered to create the cemented carbide. However, coarse grain WC powder produced from tungsten powder via high-temperature carburization generally consists of polycrystalline particles, where each WC particle is composed of multiple WC single crystals.

Figure 4 shows a scanning electron microscope image of coarse grain carbide powder with a Feret diameter of 23.20 μm. The image reveals that each WC particle contains multiple WC single crystals. Although the original powder has a coarse grain size, after grinding, the polycrystalline particles easily break down into fine single crystal particles. Consequently, the ground WC powder has a Feret diameter of only 4.85 μm. Figure 5 shows the metallographic photo of a cobalt-containing carbide with 6% Co produced using conventional carbide production processes. The average grain size of this carbide is approximately 4.0 μm.

 

How Are New Grades of Ultra-Coarse Grain Rock Drilling Cemented Carbide Developed? 6

Figure 4: SEM image of coarse grain WC powder with a particle size of 23.20 μm.

coarse grain carbide

Figure 5: Metallographic photo of WC-6% Co alloy produced from coarse grain WC powder with a particle size of 23.20 μm using conventional processing methods.

U.S. Patents 5505902 and 5529804 disclose methods for producing ultra-coarse grain cemented carbides. The methods outlined in these patents involve the dispersion and classification of coarse grain WC powder through jet milling and sieving to remove fine WC particles, selecting only the coarse-grained carbide, and then coating these WC particles with Co. Patent 5505902 utilizes the sol-gel method, where WC, methanol, and triethanolamine are mixed in a reactor. During heating, methanol evaporates, and Co precipitates onto the WC grains, forming a sol-gel.

 

Patent 5529804 employs the polyol method, where Co acetate, water, and WC are mixed and then spray-dried. The mixing process is optimized to prevent the breaking of coarse WC particles. The mixture produced using these patented methods is then subjected to conventional pressing and sintering processes to create cemented carbides with 6% Co and an average grain size of 13-14 μm, with porosity easily controlled between A02 and B02. This new carbide shows better WC matrix adjacency compared to carbides produced by traditional ball milling. Consequently, this new carbide has been successful in specific applications where conventional carbides fall short, such as in hard rock layers like granite and hard sandstone. In these cases, conventional column teeth fail due to Co dissolution at high temperatures, leading to spalling of elongated or hexagonal WC grains, and eventually, complete spalling of the drill bit within minutes, causing rapid crack propagation and subsequent fracture. In contrast, carbides produced with new technology can be used for extended periods in hard rock layers, displaying stable wear resistance without deep cracks. Due to the high adjacency of the WC matrix, the thermal conductivity of the 6% Co carbide with a WC average grain size of 14 μm can reach 134 W/m°C, which is 20% higher than that of coarse-grained carbides with the same Co content produced by traditional methods and comparable to the thermal conductivity of pure WC.

How Are New Grades of Ultra-Coarse Grain Rock Drilling Cemented Carbide Developed? 7

Application Examples of New Ultra-Coarse Grain Cemented Carbide Production Technologies

Two types of impact drilling cemented carbides were simultaneously produced using both traditional and new methods and tested in iron ore. Both samples had a WC average grain size of 8 μm, 6% Co, and 94% WC content.

Sample A: Produced using traditional ball milling, drying, pressing, and sintering processes. This carbide has a wide distribution of crystal sizes.

Sample B: The WC powder was subjected to jet dispersion and classification to remove coarser and finer WC particles, selecting 6.5-9 μm WC powder. The WC grains were pre-coated with 2% Co, and then 4% pure Co was added to achieve a 6% Co content. After wet mixing (without ball milling) to obtain the desired slurry, a thickening agent was added if necessary to prevent coarse grain WC sedimentation. The slurry was dried, shaped, and sintered, resulting in a narrower particle size distribution, with over 95% of the grains ranging from 6.5 to 9 μm. The adjacency of these carbides was measured: Sample A had an adjacency of 0.41, while Sample B had an adjacency of 0.61.

Testing was conducted in magnetite, which is prone to generating high heat and thermal fatigue. After drilling 100 μm, Sample A exhibited thermal cracking. Cross-sectional observation of the used carbide revealed small cracks extending into the carbide, damaging its microstructure and reducing its lifespan. With regrinding after every 100 μm of drilling, the carbide’s drilling lifespan was 530 meters. Sample B showed no or only minimal thermal cracking after drilling 100 meters. Cross-sectional observation showed no internal cracks, only some fractured surface grains. With regrinding after every 200 meters, the average drilling lifespan was 720 meters.

Deixe uma resposta

O seu endere?o de e-mail n?o será publicado. Campos obrigatórios s?o marcados com *

欧美精品香蕉视频在线观看-国产成人久久精品一区二区三区-亚洲国产日本在线观看-五月婷婷丁香综合在线观看| 97视频资源在线观看-国产av天堂久久精品-亚洲av一二三四区又爽又色又爽-悠悠色网视频在线精品| 精品视频人妻少妇一区二区三区-人妻中文字幕一二三区-日本老熟妇成熟老妇人-东京热国产精品二区三区| 自拍成人免费在线视频-91在线高清视频播放-国产美女口爆吞精系列-午夜福利黄片在线观看| 国产精品蜜桃久久一区二区-久久精品熟女亚洲av麻豆蜜臀-日本一区二区精品色超碰-伊人一区二区三区久久精品| 亚洲国产日韩欧美高清-偷窥偷拍一区二区三区四区-国产国亚洲洲人成人人专区-日本韩国午夜视频在线观看| 日日夜夜久久国产精品-国产男女无遮挡猛烈免费观看-在线观看热久精品视频-国产香蕉视频在线内射| 亚洲av色福利天堂在线观看-人妻少妇午夜福利视频-男人的天堂av在线视频-国内揄拍国产精品人妻一区二区| 亚洲午夜福利在线看片-草草影院在线观看国产-中文字幕在线国产有码-精品99成人午夜在线| 国产精品一区成人精品果冻传媒-日韩精品一区二区三区不长视频-欧美日韩不卡在线视频-99久久热视频在线观看| 欧美黄色在线观看免费-日本高清精品一卡二卡-日本综合精品一区二区在线-国产精品伦人一久二久三久| 国产精品久久三级精品-国产一级一片内射免费播放-一区二区三区国产精品麻豆-国产精品情侣自拍av| 亚洲免费看三级黄网站-日韩国产熟女免费精品老熟女视频-久青草视频免费在线播放-国产日韩精品久久一区二区| 亚洲精品毛片免费观看-精品一区二区三区四区激情-特黄特色大片女生高潮久久-欧美午夜福利视频自拍| 久久99国产欧美精品-深夜宅男宅女在线观看-骚虎三级在线免费播放-精品国模人妻视频网站| 日本一区二区三区视频高清-国产麻无矿码直接观看-国产精品久久久久久无-日韩精品不卡在线视频| 亚洲区一区二区三区四区-精品亚洲国产成人av-国产美腿丝袜诱惑在线观看-美女抠逼视频免费网站| 日韩在线免费av网站-免费啪视频一区二区三区在线观看-久操热在线视频免费观看-91亚洲国产成人精品性色| 黄色永久免费中文字幕-蜜臀av一区二区三区人妻在线-国产精品久久午夜伦鲁鲁-国产欧美日韩亚洲更新| 亚洲国产黄色美女视频-成人家庭影院日韩午夜-国产剧情av网址网站-91精品乱码一区二区三区| 欧美亚洲午夜综合一区二区-亚洲大香蕉视频在线观看-国产综合激情人妻91麻豆-国产精品国产三级国产专不| 精品国产一区二区三区色搞-国产极品尤物精品视频-亚洲中文字幕乱码亚洲-午夜日本福利在线观看| 欧美精品一区二区三区香蕉-国产精品黄色免费网站-蜜桃av乱码人妻一二三区-国产综合亚洲一区激情国产| 高清国产av一二三四-少妇激情高潮视频网站-被公么玩弄邻居人妻中文字幕-亚洲免费成人av在线| 台湾香港a毛片免费观看-国产美女口爆吞精的后果-亚洲天堂成人免费在线-国模在线视频一区二区三区| 综合一综合二综合久久-亚洲一区二区三区视频免费观看-亚洲国产中文字幕一区二区-日韩人妻一区二区三区蜜桃视频| 蜜臀网站视频在线播放-四虎午夜福利视频在线观看-黄色国产精品福利刺激午夜片-亚洲精品国产成人av| 欧美日韩激情免费观看-成年大片免费视频观看-俺来也去也网激情五月-在线国产精品自偷自拍| 97视频资源在线观看-国产av天堂久久精品-亚洲av一二三四区又爽又色又爽-悠悠色网视频在线精品| 国产精品久久三级精品-国产一级一片内射免费播放-一区二区三区国产精品麻豆-国产精品情侣自拍av| 日产中文字幕在线精品一区-日韩黄色特级片一区二区三区-8x8x精品国产自在现线拍-内射爆操视频在线观看| 人妻少妇一区二区三区精品-三级尤物视频在线观看-野花在线中文字幕伊人-亚洲精品一区二区播放| 四虎永久在线高清国产精品-一区二区三区日本精品视频-国产午夜福利精品久久不卡-一区二区三区国产亚洲自拍| 亚洲国内精品一区二区在线-亚洲国产成人精品青青草原-精品在线视频免费在线观看视频-亚洲美女激情福利在线| 成年深夜在线观看视频-成人国产av精品在线-av乱亚洲一区二区三区-亚洲精品综合一区二区在线| 国产福利亚洲精品精彩在线-日韩在线精品视频免费-亚洲成人国产精品av-日本不卡一区二区三区四区视频| 中文熟妇人妻又伦精品视频-久久午夜精品人妻一区二区三区-少妇被粗大猛进进出出-日韩av在线成人观看| 亚洲乱码日产精品一二三-日韩中文字幕综合在线-日韩欧美一级黄色录像-午夜福利在线视频观看| 国产深夜视频在线观看-丰满人妻熟妇乱又乱精品-青草视频在线观看资源-奇米网东京热日本人妻| 中文字幕日韩有码av-麻豆国产成人av高清在线-可以免费观看的av毛片-久久这里只有精品国产亚洲| 麻豆国产av一区二区精品-久久福利社最新av高清精品-丝袜美腿亚洲综合伊人-亚洲欧洲av一区二区三区|