Dual-phase carbide refers to a type of carbide material that contains two different forms of grains. Typically, these two forms refer to plate-like grains and columnar grains. By adjusting the manufacturing process and parameters of the alloy, the proportion and arrangement of plate-like and columnar grains can be controlled. The preparation of dual-phase hard alloy can enhance the comprehensive performance of the alloy by combining the bending strength of plate-like grains with the uniformity of columnar grains, thereby improving the mechanical properties and service life of the hard alloy.

Brief history of WC carbide

Cemented carbide, born in 1923, emerged from a legendary and awe-inspiring nation – the Germanic people.

In the late 19th century, in search of new materials to replace high-speed steel and further enhance metal cutting speed, reduce processing costs, and solve issues like tungsten wire drawing for light bulbs, people began exploring the production of cemented carbide products.

In 1893, German scientists heated tungsten trioxide and sugar together in an electric furnace to high temperatures, successfully producing tungsten carbide. They attempted to utilize its high melting point and hardness to create wire drawing dies, as a substitute for diamond materials. Unfortunately, due to the brittleness, susceptibility to cracking, and low toughness of tungsten carbide, the first exploration of cemented carbide was declared a failure.

Entering the 1920s, German scientist Karl Schroter studied and discovered that pure tungsten carbide could not withstand the intense stress changes occurring during the drawing process. Only by adding low-melting-point metals to WC could the blanks possess a certain level of toughness without compromising hardness. Schroter proposed a method of powder metallurgy, mixing tungsten carbide with a small amount of ferrous metals (iron, nickel, cobalt), then pressing and sintering the mixture at temperatures exceeding a thousand degrees Celsius, resulting in the birth of the world’s first cemented carbide.

The continuous pursuit of cemented carbide with higher hardness and greater toughness led to the development of advanced production equipment for cemented carbide. In 2005, a team led by Professor Zhu Min from South China University of Technology in China introduced cold plasma into mechanical ball milling. By ball milling W, C, and Co powders with plasma, they were able to directly sinter the pressed green compacts into high-performance cemented carbide, achieving a one-step method for preparing high-performance and controllable W-C-Co cemented carbide.

 

The production of traditional hard alloys

The production process of traditional WC-Co cemented carbide is generally complex. It involves the reduction of tungsten oxide, carburization of tungsten, wet grinding of the mixed powders, drying and granulation of the mixed powders, compact pressing, debinding, and sintering. Clearly, this production process is intricate and has a relatively long production cycle. It also requires two high-temperature processes for carburization and sintering, resulting in high energy consumption, as shown in Figure

What is 2-phase WC Carbide? 2

fig1:The production of WC-Co carbide using traditional industrial methods

 

The utilization of low-temperature plasma-assisted high-energy ball milling (dielectric barrier discharge plasma-assisted milling, abbreviated as plasma milling) equipment has enabled the efficient refinement and activation of W-C-Co powders in a short period of time. Experimental results have confirmed that the composite powder obtained after discharge plasma milling (≤3 hours), when pressed and formed, can be directly sintered into WC-Co cemented carbide at around 1390°C, as shown in Figure 2.

What is 2-phase WC Carbide? 3

fig2:The one-step method for preparing WC-Co carbide, based on dielectric barrier discharge plasma-assisted milling technology

Compared to the traditional process of cemented carbide preparation, this method (carburization-sintering one-step method) avoids the drawbacks of the two high-temperature stages in the traditional process. It enables the synthesis of WC and the densification of WC-Co alloy bodies in a single step. This method is a new approach characterized by a short preparation process, simplified procedure, and low energy consumption. By utilizing this method and controlling the grain size and morphology of WC, as well as the arrangement state of plate-like WC, a novel high-performance cemented carbide with a dual morphology and dual-scale structure has been successfully prepared.

 

The one-step method for synthesizing carbide through carbide sintering

The one-step synthesis of cemented carbide is based on the discharge plasma-assisted ball milling technology. Firstly, the original W, C, and Co powders are subjected to plasma ball milling to produce nanocrystalline W-C-Co composite powder. The ball milling time is approximately 1-3 hours. Then, the prepared composite powder is cold pressed and formed into green compacts. Finally, the green compacts are carburized and sintered in a vacuum or low-pressure sintering furnace to obtain WC-Co cemented carbide bodies in a single step, as shown in Figure 2. The cemented carbide typically prepared by this method is a high-performance nanocrystalline or ultrafine-grained WC-8Co alloy.

What is 2-phase WC Carbide? 4

Figure 3 shows the DSC curves of W-C mixed powders milled for 3 hours using conventional ball milling and plasma-assisted ball milling. After plasma-assisted ball milling, the W-C mixed powder starts to form WC at around 900°C (the new plasma-assisted ball milling equipment can achieve WC synthesis below 800°C). This temperature reduction of 300-500°C compared to conventional carburization methods significantly shortens the carbonization process by tens to hundreds of hours compared to commonly used ball milling times.

What is 2-phase WC Carbide? 5

fig4:After 3 hours of plasma-assisted milling: (a) W-C powder; (b) morphology of W-C powder after sintering at 1000°C; (c) morphology of W-C powder after sintering at 1390°C.

It is highly meaningful that WC-8Co carbide prepared using the “one-step method” process exhibits excellent mechanical properties, as shown in Figure 5.

What is 2-phase WC Carbide? 6

fig5:The mechanical properties of WC-8Co carbide prepared by plasma-assisted milling with different scales

Based on the “carburization-sintering one-step method,” by adjusting the plasma ball milling time, it is possible to obtain cemented carbide with a combination of plate-like and prismatic WC in different proportions. When an appropriate proportion of plate-like and prismatic WC is achieved, the cemented carbide exhibits improved overall performance. This is because plate-like WC possesses good flexural strength, while the presence of prismatic WC effectively avoids the issue of lower transverse rupture strength (TRS) caused by highly oriented arrangement of plate-like WC on the cross-section.

The synergistic effect of the two different forms of WC ensures the uniformity of the mechanical properties of the cemented carbide and effectively enhances its comprehensive mechanical performance. For example, for WC-8Co cemented carbide prepared by vacuum or low-pressure sintering, when the percentage of plate-like WC is around 35%, its hardness is HRA92.1, and the transverse rupture strength (TRS) is approximately 3800 MPa.

Therefore, the development of the “carburization-sintering one-step method” for preparing WC-Co cemented carbide using plasma ball milling technology enables the microstructural control of WC in multiple forms and scales. This approach facilitates the production of high-hardness and high-strength WC-8Co cemented carbide.

 

High-performance dual-phase, dual-scale WC carbide

WC crystals belong to the hexagonal crystal system. The anisotropy of the hexagonal system results in different physical and mechanical properties of WC grains in each crystallographic direction or plane. The hardness of the WC (0001) basal plane is twice that of the WC (10-10) plane. When a certain amount of plate-like WC is present in cemented carbide and its distribution state is controlled by exploiting the anisotropy of plate-like WC grain properties, dual-phase cemented carbide with better performance than conventional cemented carbide can be prepared.

In the study of the effect of WC morphology on cemented carbide performance, it has been discovered that by carefully adjusting the plasma ball milling process, control of WC morphology as prismatic or plate-like (lamellar) can be achieved in the subsequent sintering process, as shown in Figure 6.

What is 2-phase WC Carbide? 7

fig6:Cold cylindrical and plate WC morphologies of different scales prepared by plasma ball grinding

Based on this foundation, the design and preparation of dual-phase cemented carbide with dual-phase WC grains have been achieved by adjusting the processing methods. The different morphologies of WC on different cross-sections demonstrate that the morphology of WC can be controlled to be either prismatic or plate-like by adjusting the ball milling time. In the study of the effect of plate-like WC content on improving mechanical properties, the proportion of different forms of WC in the cemented carbide matrix and the arrangement state of plate-like WC have been controlled through rational design.

Currently, while maintaining high hardness in the obtained WC-8Co cemented carbide, controllability in terms of strength has been achieved. The mechanical properties of the cemented carbide mainly include hardness = 91.5 ~ 93.0 HRA, TRS = 3300 ~ 4000 MPa, and KIC = 17.5 ~ 21.5 MPa*m1/2.

As shown in Figure 7, the content of different WC morphologies in a series of dual-phase cemented carbides and the mechanical properties listed in Table 1 indicate that the typical example C1P1 of dual-phase cemented carbide has a plate-like WC content of approximately 35%. The mechanical properties of the cemented carbide on different cross-sections are as follows: hardness on the cross-section = 92.4 HRA, TRS = 3795 MPa; hardness on the longitudinal section = 92.1, TRS = 3824 MPa. This indicates that the synergistic effect of the two different forms of WC not only ensures the uniformity of the mechanical properties of the cemented carbide on different cross-sections but also effectively improves its comprehensive mechanical performance.

What is 2-phase WC Carbide? 8

fig7:Variation in the content of columnar and lamellar WC in dual-phase WC carbide

What is 2-phase WC Carbide? 9

chart1:Hardness and TRS (tensile strength) of dual-phase WC-8Co carbide (corresponding to Figure 7).

In further research on the preparation of high-content plate-like WC cemented carbide, by selecting the particle size of the original tungsten (W) powder and employing a rational preparation process, the degree of orientation of plate-like WC can be well controlled, leading to a significant improvement in the transverse fracture strength of the cemented carbide, as shown in Figure 8.

What is 2-phase WC Carbide? 10

fig8:The process route for preparing dual-scale plate-like WC-Co carbide using plasma-assisted milling technology

In the current stage of research, the WC-8Co cemented carbide containing a high proportion of plate-like WC exhibits excellent mechanical properties, with the following optimal mechanical performance: cross-sectional hardness = 92.4 HRA, transverse rupture strength (TRS) = 4083 MPa, longitudinal hardness = 92.1 HRA, and TRS = 3924 MPa.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

国产精品97一区二区三区-四虎永久免费视频播放-久久五十路丰满熟女中出-国产18日韩亚洲欧美| 中文字幕乱码亚洲精品-亚洲伊人久久大香线蕉-麻豆视传媒视频短免费网站-极品美女被后入干出水视频| 亚洲国产精品不卡毛片-青青青视频手机在线观看-在线视频中文字幕人妻-亚洲永久精品免费在线| 偷拍日韩女生厕所尿尿-水蜜桃一区二区三区四区-亚洲成人色黄网站久久-久久久国产综合午夜精品| 97资源视频在线观看-青草视频在线免费播放-最新日韩中文字幕在线播放-成人国产av精品麻豆网站| 少妇被搞高潮在线免费观看-亚洲av成人精品小宵虎南-日韩性生活免费看视频-日韩黄色大片在线播放| 青青青视频蜜桃一区二区-粗大挺进人妻中文字幕-国产小视频在线看不卡-国产精品一区免费在线观看| 日本岛国三级黄色录像-日韩久久成人免费电影-中文字幕日韩专区一区二区-国产成人大片在线播放| 精品三级国产三级在线专区-精品一区二区三区视频观看-在线精品日韩亚洲欧一二三区-美女高潮无套内射视频免费| 国产成人综合中文字幕-中文字幕午夜五月一二-在线视频精品一区二区三区-久久96精品国产亚洲av蜜臀| 日韩中文字幕精品人妻-国产欧美亚洲91在线-亚洲欧美激情第一欧美精品-精品视频美女久久久中文字幕| 亚洲欧洲av一区二区久久-日本丰满熟妇中出在线-欧美一区二区三区人妻少妇-日韩成人av免费在线| 精品国产人成亚洲区中文久久-欧美日韩夫妻性生活视频-亚洲欧美日韩高清专区一-国产精品无套内射后插| 与老熟女激情av国产-91午夜福利在线观看视频-国产特级黄片免费观看-精品亚洲熟妇中文字幕| 国产精品国产三级在线试看-亚洲男人天堂一区二区在线观看-风韵丰满熟妇啪啪区99杏-最近中文字幕日韩有码| 国产精品人人爱一区二区白浆-中文字幕一区二区三区人妻精品-91人妻在线欧美精品不卡-好吊视频一区二区三区在线| 国产在线一区二区三区不卡-久久精品女人毛片水多国产-无人区一码二码三码四码区免费-日韩亚洲国产成人在线| 台湾香港a毛片免费观看-国产美女口爆吞精的后果-亚洲天堂成人免费在线-国模在线视频一区二区三区| 无套内射在线免费观看-亚洲日本va中文字幕久-日韩免费人妻av一区二区三区-热久久国产最新地址获取| 久久亚洲国产高清av一级-免费国产精品自偷自偷免费看-日本a级特黄三级三级三级-欧美日韩一区二区中文字幕高清视频| 国产一区二区在线观看不卡-日本高清中文字幕有码在线-日本女优在线观看一区二区三区-在线观看免费四虎av| 久热视频在线免费观看-亚洲一区二区日韩综合久久-免费观看在线观看青青草视频-精品一区二区亚洲一区二区血炼| 亚洲国产日韩欧美高清-偷窥偷拍一区二区三区四区-国产国亚洲洲人成人人专区-日本韩国午夜视频在线观看| 91精品在线播放黑丝后入-97免费在线播放视频-av网站天堂网国产av-亚洲熟妇乱色一区二区三区| 国产成人综合激情婷婷-亚洲国产综合在线观看不卡-色综网久久天天综合狼人-亚洲av高清在线不卡| 日本一区二区三区最新章节-香蕉av久久一区二区三区-久久久国产亚洲精品视频-国产伦精品一区二区三区精品视频| 成人精品一区二区三区久久-中文字幕乱码亚洲无线三区-亚洲精品亚洲人成人网-中文字幕五月久久婷热| 欧美亚洲国产另类在线-九九热精品在线免费视频-日本高清有码在线一区-青草第一视频在线观看| 日韩一卡二卡在线播放-亚洲国产精品懂色av-青青热久免费精品视频在-久久精品中文字幕一区二区三区| 久久97久久97精品免视看秋霞-黄片av毛片在线免费观看-日韩av高清不卡免费观看-成人午夜福利视频观看地址| 女同精品女同系列在线观看-亚洲av不卡一区二区三区四区-亚洲不卡一区三区三州医院-中文字幕亚洲人妻系列| 免费十八禁一区二区三区-国产精品一区二区三区99-在线一区二区三区男男视频观看-精品欧美一区二区三区人妖| 国产精品一区二区在线观看免费-日本老熟妇色视频免费-亚洲码国产精品高潮在线-日韩一区二区三区日韩| 久久都是精品久久都是精品-精国精品一区二区成人-亚洲品质自拍在线观看-中文 字幕乱码高清视频| 久久国产精品一品二品-国产二区中文字幕在线观看-极品性感尤物少妇粉嫩逼-亚洲成人av男人的天堂网| 亚洲av色香一区二区三含羞草-av毛片在线观看网站-中文字幕一区二区人妻中文字-91精品人妻日韩一区二区| 亚洲视频在线观看第一页-精品偷拍另类欧美日韩-日韩高清在线一区二区三区-久久天天操狠狠操夜夜av| 午夜性福福利视频一区二区三区-午夜福利在线看片在线-欧洲内射免费人文艺术-亚洲天堂成人av在线| 日韩三级在线视频不卡-国内自拍色第一页第二页-96热久久这里只有精品-日韩精品有码一区二区三区久久久| 四只虎视频大全免费观看-日本黄色激情免费网站-免费岛国大片在线播放-国产午夜福利在现观看| 国语对白高清在线观看-久久av精品一区二区三区-日韩在线中文字幕不卡-免费视频成人高清观看在线播放|