This article analyzes the reasons for the problems encountered during the external cylindrical grinding of graphite material components. Graphite is a black non-metallic material with a low density of 2.25g/cm3 [1]. Due to its advantages such as high-temperature resistance, self-lubrication, corrosion resistance, light weight, and good plasticity, it has found widespread applications in industrial production. Graphite products generally have stringent quality requirements. However, the inherent characteristics of graphite materials make them prone to various issues during processing, such as the occurrence of excessive ovality, dimension deviations, and defects in the processing surface when grinding the external cylindrical shape. These issues can lead to substandard or even scrapped machining products.

?

The problems encountered during external cylindrical grinding

Clamping deformation

Due to the characteristics of the component’s external dimensions and its inherent flexibility, slight variations occur in the components during clamping, which subsequently affects product quality, as illustrated in Figure 1.

Fig.1 parts awaiting external cylindrical grinding
Fig.1 parts awaiting external cylindrical grinding

the roundness and coaxiality of parts

The two machining reference points for affecting the roundness and concentricity of the component are the inner bore and the core shaft. The inner bore of the component has an interference fit with the small tapered core shaft. Wear of the core shaft or poor contact between the tip and the center hole may cause excessive runout. In the previous machining step, the inner bore was processed using a lathe, and deformation during clamping could result in the inner bore taking on an elliptical shape, thereby affecting the machining accuracy of the outer circle.

The size of the parts

Graphite material has significant toughness, and when graphite components are clamped on the core shaft, the conical shape of the core shaft causes the component to be stretched by the core shaft, resulting in deformation. This deformation leads to the actual dimensions of the component being smaller, causing an excessive tolerance.

Various defects occur on the surface of parts

During the grinding process of graphite material components, due to their relatively soft texture, various defects can occur on the component’s surface due to factors such as abrasive particle size and grinding methods:

1Polygonal defects: There are evenly spaced straight-line marks along the axis direction on the component’s surface.

2Spiral defects: The grinding surface exhibits a spiral pattern.

3Scratches or grooves: Noticeable incised grinding marks appear on the surface, varying in size and length.

?

Rozwi?zania

Choice of grinding wheel

The characteristics of the grinding wheel (abrasive material, grain size, hardness, bonding agent, and wheel structure, etc.) play a crucial role in the quality of grinding the external circumference of graphite material components. If the grinding wheel selection is inappropriate, it becomes difficult to achieve the required surface roughness of the graphite component. Furthermore, the cutting performance of the grinding wheel needs to be ensured. When processing graphite components, choosing a slightly harder grinding wheel with abrasives that do not easily detach can prevent loose abrasives from adversely affecting the machining surface while maintaining the sharpness of the grains. The machining process of the components is illustrated in Figure 2.

Fig.2 The processing of external cylindrical grinding
Fig.2 The processing of external cylindrical grinding

Improve cylindrical grinding method

Generally, processing is carried out using rough and finish grinding methods. During rough grinding, a large amount of stock is left on the component, and transverse feeding is employed. Due to the significant contact area between the grinding wheel and the graphite component, heat generation during grinding is common, so adequate cooling is essential during rough grinding. For finish grinding, longitudinal feed grinding is used, with transverse feeding during the grinding process. The grinding wheel removes a smaller amount of material, effectively ensuring the machining precision and dimensional requirements of the component.

Improve method of mounting parts

Generally, the outer diameter is machined using a tapered mandrel with an interference fit between the graphite component and the mandrel, so the clamping force should be appropriate. The clamping of the component is shown in Figure 3. Typically, a larger clamping force is used during rough grinding because, during this process, the feed rate is relatively high, and the component experiences compression. Moreover, the grinding forces acting on the component are significant. Using a larger clamping force helps prevent relative movement between the component and the mandrel. During finish grinding, when there is no relative movement between the component and the mandrel, it’s better to have a smaller clamping force. This is to prevent elastic deformation of the graphite component due to being expanded by the mandrel, which could affect the component’s dimensions. The interference fit is generally 0.005 to 0.1mm during rough grinding and 0.003 to 0.005mm during finish grinding.

Fig.3 Clamping
Fig.3 Clamping

 

Graphite products processing examples

The component material is grade M125P, characterized by its lightweight and low density, making it a brittle material. The machining blueprint requires a coaxiality of 0.01mm between the inner hole and outer diameter, with a surface roughness value of Ra=0.8μm. It is processed using an M1420A external cylindrical grinder, following the RT Inspection 03 table for size matching. Gap values are calculated and filled into the RT-40 table, and the machining is carried out with a mandrel. The post-grinding component is shown in Figure 4.

Fig.4 The parts after grinding
Fig.4 The parts after grinding

 

Actual process analysis

The two machining benchmarks for coaxiality are the component’s inner bore and the outer diameter of the mandrel. Wear on the mandrel or poor contact between the tip and the central hole can cause excessive runout. In the previous process, the component’s inner bore was machined using a lathe, and there was deformation during clamping, which could result in the inner bore being elliptical and thus affecting the machining of the outer diameter.

Elastic deformation of the component and the clamping force during fixation can affect machining precision and lead to measurement errors. The greatest challenge in machining is the surface roughness of the graphite component’s outer diameter. Since graphite is a non-metallic material, the mixture of abrasive particles from the grinding wheel and the cutting fluid can scratch the surface of the workpiece. Tiny particle impurities in the circulating cutting fluid can also enter the grinding area, causing scratches. Wheel dulling can result in multiple edges or spiral thread defects on the workpiece’s surface.

Solutions for the practical instance

Guarantee the coaxiality of the parts

The mandrel is measured with a lever dial indicator on an offset indicator before use to ensure that the runout of the outer diameter at both ends of the mandrel to the center hole is less than 0.005mm.

Guarantee the?size of the parts

The machining of the component is divided into rough and finish grinding stages.

During rough grinding, surface roughness and deformation are not considered; the goal is to leave an allowance for subsequent finish grinding. The machining process adopts a positioning cutting method with a relatively large feed rate, and it is carried out in multiple passes with a feed rate controlled between 0.01 to 0.02mm/r. The clamping force between the component and the mandrel is slightly greater, with an interference fit of approximately 0.005 to 0.01mm, which helps improve work efficiency.

During finish grinding, the component’s dimensions are measured first. If the component has deformed and exhibits an elliptical shape or if the cylindricity exceeds 0.01mm, it undergoes a reaming process to ensure dimensional accuracy. The clamping force during this stage should be moderate, with an interference fit between the mandrel and the component controlled within the range of 0.003 to 0.006mm. This minimizes elastic deformation of the clamped component, ensuring geometric tolerances are maintained. Grinding is performed using a reciprocating feed method, with a feed rate ranging from 0.001 to 0.005mm/r. This results in a smaller depth of cut and less grinding material, reducing the duration of pressure application during grinding and allowing for more precise size matching.

Guarantee the surface roughness of the parts

During finish grinding, the wheel wear is minimal, and typically, removing 0.05mm of material is sufficient to restore the wheel’s cutting performance. The correction speed should be slower, around 150 to 200mm/min. Finally, a polishing step is performed to remove any individual protrusions and loose abrasive grains from the wheel’s surface.

selection suitable cutting fluid

During the machining of graphite material components, it’s essential to ensure that the cutting fluid is clean. The machine tool should be equipped with a filtration system to prevent abrasive particles dislodged from the wheel from scratching the workpiece surface or tiny particle impurities from mixing into the circulating cutting fluid and entering the grinding zone.

Fixed value measurement

After the graphite components are finished machining on the machine tool, they need to undergo a constant temperature setting, and measurements are taken once the components have stabilized. Subsequently, gap values are calculated based on the corresponding table and recorded.

Wniosek

This article has addressed the issues encountered during the external cylindrical grinding of graphite components and provided solutions while summarizing and sharing experiences and techniques in grinding processes. When machining graphite material components, it is crucial to conduct a careful process analysis, taking into account the material’s inherent characteristics and the requirements of the drawings. Proper fixture selection, grinding wheel choice, and grinding methods should be employed to address problems such as clamping deformation, dimensional deviations, and surface defects in order to produce high-quality products.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

久99久热这里只有精品-日韩av一区二区三区播放-天堂日韩av在线播放-中文字幕被侵犯的人妻| 亚洲av色香一区二区三含羞草-av毛片在线观看网站-中文字幕一区二区人妻中文字-91精品人妻日韩一区二区| 亚洲激情文学国产激情-一本色道久久综合亚洲精品高-国产精品高清在线播放-九九热视频在线观看精品| 日本一区二区三区欧美精品-农村少妇真人毛片视频-亚洲av乱码专区国产乱码-跨年夜爆操极品翘臀日韩| 国产在线观看av自拍-成人自拍小视频在线看-十八禁网站在线免费观看-丰满的熟妇露脸大屁股| 中出少妇中文字幕一区二区三区-九九久久精品国产亚洲-美女免费是黄的一区二区av-日本在线视频观看91| 亚洲天堂久久中文字幕-高清国产一级片免费看-伊人狼人综合日日夜夜-手机看片高清国产日韩| 日本一区二区三区三级视频-亚洲国产精品一区二区久-蜜桃视频网站免费观看-在线视频中文字幕一区二区| 日韩精品少妇一二三区免费av-麻豆蜜桃av免费观看-亚洲欧洲日韩一区二区中文字幕-久久九特黄的免费大片| 国产激情在线观看视频-久久久精品国产视频在线-亚洲国产成人精品在线-亚洲乱码国产乱码精品视频| 男人天堂色男人色偷偷-国产内射在线干得爽到语无次-国产成人亚洲欧美二区综合-精品欧美高清视频观看| 日本亚洲午夜福利视频-欧美日韩高清精品一区二区-av成人免费在线视频-日韩精品一区二区三区费暖暖| 高清有码在线观看日本-精品少妇人妻一区av-色综合久久成人综合网-久久久国产精品人妻一区二区三区| 日韩精品一区二区三中文字幕-欧美亚洲日本精品一区二区-日韩av亚洲在线观看-亚洲欧美国产日韩激情| 国产在线一区二区三区蜜桃-在线免费观看青青草视频-精品91麻豆免费观看-亚洲福利网址在线观看| 日韩熟女av在线观看-中文字幕人妻丝祙乱一区三区-亚洲国产精品第一区二区三区-欧美制服丝袜一区二区三区| 日本一区二区免费电影院-亚洲精品成人av观看-国产级一片内射视步页-日韩高清在线亚洲专区视频| 亚欧曰中文字幕av一区二区三区-最新国产情侣在线视频-黄片大全视频免费在线观看-久久超级碰碰碰一区二区三区| 亚洲av优女天堂熟女美女动态-激情免费视频一区二区三区-一区二区三区国产日韩av-最新国产内射在线免费看| 男女啪啪动态视频免费-日韩精品一区二区高清-日韩在线有码中文字幕-日本免费高清一区二区三区视频| 四虎永久在线精品免费青青-久久久久久久 国内精品-国产精品四虎永久免费视频-男人天堂av免费观看| 精品人妻在线一区二区三区-国内av在线免费观看-亚洲av影片一区二区三区-久久精品女同亚洲女同13| 99一区二区三区精品人妻-国产污视频网站在线观看-伊人激情av一区二区三区-天堂av大片免费观看| 欧美亚洲国产另类在线-九九热精品在线免费视频-日本高清有码在线一区-青草第一视频在线观看| 亚洲天堂av资源在线-四虎永久免费在线观看国产-久久这里只有精品人妻-欧美黄色三级经典精品| 中文字幕av东京热久久-国产精品日韩精品最新-亚洲激情av免费观看久久-亚洲第一精品国产网站| 国产一级r片内射视频播放-中文字幕最新精品资源-久久青青草原精品国产麻豆综合-深夜成人在线免费视频| 亚洲精品色国语对白在线-黄片毛片av在线免费观看-久久精品有码av天堂-日韩一区二区三区高清视频| 国产亚洲精品首页在线播放-中文字幕国产av中文字幕-日本免费午夜福利视频-亚洲伦理一区二区三区四区| 黄色av日韩在线观看-偷拍自拍在线免费视频-色偷偷偷亚洲综合网另类-国产成人免费综合视频| 综合一综合二综合久久-亚洲一区二区三区视频免费观看-亚洲国产中文字幕一区二区-日韩人妻一区二区三区蜜桃视频| 密臀av免费在线观看-日韩欧美中文字幕美利坚-av黄色在线观看一区二区三区-日韩性做爰片免费视频看| 亚洲一区二区欧美日韩-亚洲精品四虎在线观看-国产夫妻在线视频播放-激情人妻中文字幕中字福利在线| 国产色片地址网日本激情-国产自偷在线拍精品热不卡-国产精品自产拍蜜臀av在线-成人区人妻精品一区二区三区| 日韩有码中文字幕在线视频-草草影院国产在线观看-日韩中文字幕有码午夜美女-亚洲第二十页中文字幕| 精品国产精品久久一区免费式-男女高清无遮挡免费视频-av男人的天堂一区二区三区-免费观看视频网站97| 女人毛茸茸的外阴视频-成人激情午夜福利视频-国产精品性色一区二区三区-国产中文字幕欧美激情| 亚洲人妻av在线播放-日韩午夜短视频在线观看-91精品久久午夜中文字幕-亚洲熟伦熟女新五十熟妇| 四虎永久精品免费在线-国产一级片内射在线播放-国产精品无套粉嫩白浆在线-色综合综合色综合色综合| 亚洲av优女天堂熟女美女动态-激情免费视频一区二区三区-一区二区三区国产日韩av-最新国产内射在线免费看| 蜜臀一区二区在线观看视频-亚洲一区二区国产精品视频-国内精品国产三级国产a久久-婷婷久久亚洲中文字幕|