Mining pick is one of the vulnerable parts in coal mining and roadway driving machinery, and it is the main tool for coal falling and coal breaking. Its performance directly affects the production capacity of coal mining machinery, power consumption, working stability and the service life of other related parts. With the increase of people’s demand for energy, especially for coal, in order to improve the mining efficiency, the power of the shearer is increasing, and the quality of the pick is required to be higher and higher. As the material of the shearer pick, it is required to have higher strength, hardness and wear resistance, bending strength and corrosion resistance.

Working process of shearer pick

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 2

Under the action of the front edge of the pick, the coal is broken and the large block is peeled off at the same time. At the moment when the tip contacts the coal, there are elastic and plastic deformation in the contact range of the tip. With the increase of the contact stress, when the strength limit is exceeded, the core is crushed into very fine powder to form a dense core, which is composed of the crushed coal under pressure. With the advance of the cutting tool, the dense core gradually grows and accumulates energy, and the cutting resistance also increases. The dense core compresses the front coal area and makes this part produce elastic deformation. Because the ore body around the dense core forms the stress state area, it actually plays a role in changing the geometry of the pick cutter head. When the contact stress of the cutter tip increases to the limit value, the dust in the area before the dense core ejects at a high speed, driving the small pieces to peel off.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 3

Failure form

The main failure forms are the invalidation of alloy cutter head, chipping of cutter head, wear of alloy cutter head and gear body. In some working conditions, the failure of pick is often caused by the fracture of gear body. As the mechanical performance of the pick body directly affects the service life of the pick, it is of positive significance to select the material and effective heat treatment method of the pick body reasonably to reduce the wear and fracture of the pick, reduce the consumption of the pick of the shearer, improve the operation rate of the shearer and increase the comprehensive economic benefits of the production of the shearer.

Wear and fracture failure

In the process of cutting coal seam, the pick has strong friction and abrasive wear with the coal seam. The most stressed point of the pick is at the head of the working part of the pick, where the wear is the most serious, resulting in the wear and failure of the pick pants. In the actual coal production, about 50% of the pick failure is caused by wear.

Breaking and invalidation of cemented carbide tooth head

The invalidation of cemented carbide is related to the hardness of ore in coal and rock: when the pick cuts coal and rock, if the hard ore in coal and rock is encountered, the cutter head is in the state of high-pressure stress, and it will bear high shear stress at the place where the contact between the cutting edge and coal and rock is poor, and it is in the state of tensile stress. When the tensile stress exceeds the strength limit of the alloy, the cutter head will break.

related to the poor brazing quality of tooth head.

For example, there are sand inclusions and microcracks in the weld, which cause the shear strength of the weld to be low. The abscission of cemented carbide is also related to the unreasonable size of weld gap. The use of less solder during brazing results in the loosening of cemented carbide head and the abscission of tooth head.

related to the low hardness and poor wear resistance of the working part

From the point of view of the material of the pick pant body, the reason for the invalidation of the carbide cutter head is related to the low hardness and poor wear resistance of the working part of the pick magazine body. The excessive wear of the part of the pick supporting the carbide results in the insufficient supporting force and the invalidation of the carbide. Therefore, by improving the hardness of the working part of the pick and the quality of brazing, the invalidation of cemented carbide can be avoided.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 4

Performance improvement method

1. According to the hardness index of coal and rock, the corresponding grade of alloy cutter head is selected. Generally, the compressive strength of coal or coal rock roadway can be selected with less Co. the compressive strength of roadway surrounding rock should adopt the use of advanced technology such as limited or manufacturing composite alloy material spraying to improve the impact resistance.

2. The manufacturing process shall be in strict accordance with the design requirements, to ensure the matching between the pick and the gear holder, to ensure that the tool can rotate freely in the gear holder, to avoid the phenomenon of eccentric wear, the automatic grinding function, to maintain the normal wear of sharp blade and even cutting teeth, in the cut state. Brazing and heat treatment process. Brazing and heat treatment process is one of the key technologies for cutting quality of pick.

3. A layer of niobium carbide hard alloy is deposited on the surface of the coal pick steel machine by using the hardfacing technology to obtain the hardfacing wear-resistant layer with metallurgical structure with the base. Niobium carbide is distributed on the iron-based martensite and retained austenite intensively in the trading net of Chinese shearer, which protects the collective from wear. The Hardmetals with high hardness in the hardfacing layer and a large number of metallographic structures that play the role of wear-resistant framework make the hardfacing layer have high wear-resistance.

4. Thermal spraying can heat a linear or powdery material to a melting or semi melting state and accelerate the formation of high-speed droplet by means of heat sources such as flame, arc or plasma, spray to the substrate to form a coating on it, which can strengthen the surface of the material and improve its wear-resistant and corrosion-resistant properties.

5. Plasma cladding is a new material surface modification technology which uses plasma beam as heat source to obtain excellent wear resistance, corrosion resistance, heat resistance, impact resistance and other properties of metal surface. Plasma cladding is a rapid non-equilibrium solidification process, which has many strengthening effects such as supersaturated solution strengthening, dispersion strengthening and precipitation strengthening.

6. The brazing and heat treatment process of the pick is one of the key technologies to ensure the quality of the pick. At present, the brazing and heat treatment of pick are integrated technology. It is heated by vacuum furnace, so that the brazed pick can be directly quenched without air cooling, and the brazing and heat treatment can be completed once. It can avoid the oxidation phenomenon of the traditional brazing surface contacting with the air, ensure the direct contact between the melted solder and the brazing surface, and ensure the welding quality; at the same time, because the brazing and heat treatment are completed once, it can avoid the embrittlement of the alloy head and the reduction of the weld strength caused by the two heating.

在线视频观看一区二区三区-日韩成年人高清精品不卡一区二区-成人深夜节目在线观看-亚洲精品中文字幕一二三| 九九热在线视频中文字幕-午夜激情在线观看不卡-国产精彩激情视频在线观看-人妻丰满熟妇九九久久| 亚洲高清精品偷拍一区二区-日本午夜理论一区二区在线观看-乱天堂黑夜的香蕉颜姿-天堂精品人妻一卡二卡| 日韩av观看一区二区三区四区-美丽的蜜桃3在线观看-久久人妻少妇嫩草av-欧美亚洲另类久久久精品| 国产精品国产三级在线试看-亚洲男人天堂一区二区在线观看-风韵丰满熟妇啪啪区99杏-最近中文字幕日韩有码| 日韩视频精品在线播放-国产91亚洲精品久久-亚欧洲乱码视频在线观看-亚洲国产成人91精品| 91精品久久综合熟女-日产精品毛片av一区二区三区-国产精品永久在线播放-一区二区中文字幕在线视频| 91国际精品麻豆视频-蜜臀av国产在线观看-av一区二区三区精品-人妻精品一区二区三区av| 日韩视频精品在线播放-国产91亚洲精品久久-亚欧洲乱码视频在线观看-亚洲国产成人91精品| 国内国产精品国产三级-美女性爽潮喷白丝小仙女-国产精品自拍露脸在线-国产精品亚洲综合日韩| 国产精品97一区二区三区-四虎永久免费视频播放-久久五十路丰满熟女中出-国产18日韩亚洲欧美| 精品国产乱码一二三区在线-精品国产一区二区在线视-国内男女精品一区二区三区-亚洲中文字幕国内精品| 国内外成人综合免费视频-久久国产精品99久久蜜臀-大三美女口爆吞精视频-亚洲国产一区二区精品性色| 日韩有码中文在线视频-少妇我被躁爽到高潮在线观看-精品丰满人妻一区二区三区-亚洲天堂高清在线播放| 国产一级r片内射视频播放-中文字幕最新精品资源-久久青青草原精品国产麻豆综合-深夜成人在线免费视频| 免费在线观看午夜视频-成人性生交大片免费网站-国产一区二区精品久久胖女人-亚州综合国产精品天码av| 开心五月激情综合久久爱-国产精品深夜在线观看-91亚洲国产成人精品一区.-精品亚洲国产成人性色av| 国产高清三级自拍视频-最近日本免费播放视频午夜-日本女优一级片中文字幕-在线播放深夜精品三级| 熟女国产精品一区二区三-一区二区三区av这些免费观看-精品国产一区二区二三区在线观看-国产精品一品二区三区日韩| 欧洲熟女乱色一区二区三区-人妻中文字幕一区二区在线视频-亚洲码欧洲码一区二区三区四区-日本片在线美女视频骚货| 岳的大肥屁熟妇五十路99-偷拍美女解手视频精品-日韩欧美一区二区三区精品-亚洲国产精品成人自拍| 欧美精品香蕉视频在线观看-国产成人久久精品一区二区三区-亚洲国产日本在线观看-五月婷婷丁香综合在线观看| 亚洲国产成人不卡高清麻豆-精品国产精品三级在线专区-亚洲欧美国产日韩一区-亚洲高清日本一区二区| 久久精品蜜桃一区二区三区-久久99亚洲精品久久-激情文化变态另类快播-国产成人免费永久在线平台| 黄色av日韩在线观看-偷拍自拍在线免费视频-色偷偷偷亚洲综合网另类-国产成人免费综合视频| 国产精品中文字幕在线一区-国产成人美女精品自在拍av-密桃av一区二区三区四区-女优免费中文字幕在线| 日韩欧美国产在91啦-激情偷拍自拍在线观看-一本大道久久香蕉成人网-亚洲精品中文字幕观看| 能看免费欧美一级黄片-男女视频网站免费精品播放-日本高清在线一区二区三区-熟女少妇免费视频网站观看| 国产韩国精品一区二区三区-久久精品人妻一区二区三区av-黄片视频在线观看欧美-国产成人自拍在线视频| 九九久久只有精品视频-精品女厕偷拍一区二区三区-欧美超乱碰精品综合在线-av中文字幕少妇人妻| 精品国产亚洲av蜜臀-欧美亚洲伦理在线视频-久久亚洲国产成人影院av-国产精品99蜜臀久久不卡二区| 欧洲激情综合啪啪五月-国产精选三级在线观看-七七久久成人影院网站-男人深夜福利在线观看| 九九热在线精品视频免费-日韩高清免费在线视频-熟女快要高潮了在线观看-亚洲午夜福利视频一级| 激情视频在线观看国产一区-日韩高清在线视频一区免费观看-国产白丝精品在线观看-色偷偷伊人大杳蕉综合网| 久热免费观看视频在线-久久精品免费看国产成人-91极品女神嫩模在线播放-青草视频在线观看久久| 免费手机在线观看bbb视频-国产欧美亚洲精品第1页青草-国产黄a三级三18级三级看三级-宅男视频在线观看一区二区三区| 国产精品一区二区三区四区-日本毛茸茸的丰满熟妇-中文字幕久久中文字幕久久-国产成人三级一区二区在线观看| 日韩欧美熟妇在线观看-在线视频一区二区三区在线观看-欧美黄色在线观看网站-国产精品综合亚洲91| 91精品18国产在线观看-午夜福利原创精品视频-欧美日韩在线亚洲另类-欧美日韩亚洲国产综合在线| av资源视频在线观看-最新福利一区二区三区-极品白嫩粉嫩美女国产-久久精品国产亚洲av麻豆软| 精品国产一区二区三区吸毒-国产精品一品二区精品网站-偷拍美国美女厕所撒尿-日韩精品在线视频一二三|