The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 1

Spherical Cast Tungsten Carbide Powder is a novel type of highly wear-resistant ceramic particle material. Compared to traditional tungsten carbide, spherical cast tungsten carbide possesses two significant advantages. Firstly, it has a regular spherical appearance with good powder flowability and wetting properties. When used as an additive particle, it exhibits excellent compatibility with the surrounding structure, reducing stress concentration. Secondly, the internal structure of the tungsten carbide particles is dense, exhibiting good toughness, fine grain size, high hardness, and excellent wear resistance as a coating. It is less prone to fracture under load.

Due to its outstanding performance, spherical cast tungsten carbide powder is gradually replacing traditional tungsten carbide powder in surface protection applications for mining machinery, petroleum machinery, construction industry, and foundries. It significantly enhances the wear resistance, corrosion resistance, and oxidation resistance of components, thereby extending their service life.

The chemical composition, microscopic morphology, microstructure, microhardness, and other powder properties of spherical cast tungsten carbide powder prepared by different methods will be investigated below.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 2

1.Chemical composition of sample carbide powder

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 3

The table above shows the chemical composition of spherical cast tungsten carbide powder samples prepared by different methods. It can be observed that the main components of spherical cast tungsten carbide powder are tungsten (W) and carbon (C), with trace amounts of iron (Fe), vanadium (V), chromium (Cr), and niobium (Nb). The ideal composition of spherical cast tungsten carbide should consist of eutectic WC and W2C phases, with a eutectic temperature of 2525 ℃ and a carbon content of 3.840% (mass fraction) at the eutectic point. From the data in the table, it can be seen that the spherical cast tungsten carbide powder prepared by the plasma rotating electrode atomization method has the smallest deviation from the theoretical carbon content and the lowest free carbon content. On the other hand, the powder obtained from the induction melting and atomization method shows the largest deviation from the theoretical carbon content, with a difference of 0.170% (mass fraction). This is likely due to the use of graphite tube heating in the induction melting process, which can increase the carbon content. Therefore, compared to other methods, the plasma rotating electrode atomization method can more accurately control the carbon content of spherical cast tungsten carbide powder, preventing over-eutectic and sub-eutectic reactions caused by carburization and decarburization, and achieving a near-perfect eutectic microstructure. This is crucial for improving the microstructure and properties of spherical cast tungsten carbide.

2.Microscopic morphology

fig1.The microstructure of spherical cast tungsten carbide powder samples
fig1.The microstructure of spherical cast tungsten carbide powder samples

The figure above shows the microstructure of spherical cast tungsten carbide powder prepared by different methods. It can be observed that the spherical cast tungsten carbide powder obtained from all three methods exhibits a regular and smooth near-spherical shape.

The cross-sectional images of spherical cast tungsten carbide powder
fig.2 The cross-sectional images of spherical cast tungsten carbide powder

The figure above shows cross-sectional photographs of spherical cast tungsten carbide powder prepared by different methods. From (a) and (b), it can be observed that the particles of spherical tungsten carbide powder prepared by plasma rotating electrode atomization method have a dense internal structure with almost no defects. However, from (c) and (d), it can be seen that spherical tungsten carbide powder prepared by plasma melting and atomization as well as induction melting and atomization methods have some noticeable pores or hollow particles within their internal structure. The main reason for this is that the crushed tungsten carbide powder used as raw material in the above-mentioned methods may contain residual pores from the casting process. During the short-duration plasma or induction heating process, it becomes challenging for the internal part of the crushed tungsten carbide powder to fully melt, resulting in the presence of some pores within the particles.

3.Microstructure

the microscopic structure of spherical cast tungsten carbide powder samples
fig3. the microscopic structure of spherical cast tungsten carbide powder samples

The figure above displays microscopic images of the microstructure of spherical cast tungsten carbide powder particles prepared by different methods after corrosion. It can be observed that the internal structure of the particles in all three methods primarily consists of a typical fine needle-like eutectic structure of WC and W2C phases. Compared to plasma melting and atomization and induction melting and atomization methods, the eutectic microstructure of spherical cast tungsten carbide powder obtained by plasma rotating electrode atomization method appears to be finer and denser. This is because, in contrast to plasma melting and atomization and induction melting and atomization methods, plasma rotating electrode atomization method fully melts the tungsten carbide raw material rod and rapidly solidifies it under the centrifugal force. The higher undercooling during the crystallization of the molten tungsten carbide results in more rapid nucleation and a greater number of crystal nuclei formation, leading to a finer eutectic microstructure.

4.Microhardness

The table below shows the average microhardness of spherical cast tungsten carbide powder prepared by different methods. It can be observed that the microhardness of the spherical cast tungsten carbide powder obtained from all three methods is above 2800 HV0.1. Among them, the powder produced by the plasma rotating electrode atomization method exhibits the highest microhardness, reaching 3045 HV0.1. This is mainly due to the finer and denser eutectic microstructure within the spherical cast tungsten carbide powder obtained by the plasma rotating electrode atomization method.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 4

5.Other physical properties

The table below presents the flowability and tap density values of spherical cast tungsten carbide powder prepared by different methods. It can be observed that the powder obtained from the plasma rotating electrode atomization method has the poorest flowability and the lowest tap density. On the other hand, the powder obtained from the induction melting and atomization method exhibits the best flowability and the highest tap density.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 5

Wniosek

(1) The spherical cast tungsten carbide powder prepared by the plasma rotating electrode atomization method exhibits the smallest deviation from the theoretical carbon content and eutectic carbon content, with the lowest free carbon content and relatively low impurity content.

(2) The internal structure of the spherical tungsten carbide powder particles obtained by the plasma rotating electrode atomization method is dense, with almost no defects. The eutectic microstructure is finer and denser. On the other hand, the particles obtained by plasma melting and atomization as well as induction melting and atomization methods show some noticeable pores or hollow particles within their internal structure.

(3) All three methods result in spherical cast tungsten carbide powder primarily consisting of WC and W2C phases.

(4) The microhardness of the spherical cast tungsten carbide powder obtained by all three methods is above 2800 HV0.1. Among them, the powder produced by the plasma rotating electrode atomization method exhibits the highest microhardness, reaching 3045 HV0.1. The powder obtained by the induction melting and atomization method shows good flowability and the highest tap density.

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 6

The performance study of spherical cast tungsten carbide powder prepared by the 3 methods 7

 

 

 

 

lipiec 16, 2023

Hello. I work in the aviation sector and we are metal strip drawing SS aviation grade metal and cannot seem to find a carbide that gives us the toughness and long wear properties that normal carbide would provide with regular tungsten carbide used in metal drawing of softer materials?Would you have a supplier list of companies that provide this new type of carbide? Regards

sierpień 3, 2023

Hello Dale,
Thank you for leaving a comment!
Could you please send us an inquiry to [email protected]?
Z powa?aniem,

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

国色天香精品亚洲精品-日韩精品电影免费观看-亚洲精品中文字幕综合-成人午夜视频福利在线观看| 久久精品国产欧美日韩热-久久综合色一综合色88-特西西日本午夜人体艺术-97中文字幕在线视频| 天堂av免费资源在线观看-青春草在线视频播放免费观看网站-亚洲精品中文字幕久久桃色-亚洲成人有码免费在线| 亚洲国产成人精品毛片九色-成年片黄色大片品赏网-亚洲男人天堂色噜噜av-人妻免费精品久久一区| 久久夜色国产精品亚洲-国产视频一区二区三区免费观看-亚洲一区二区成人在线观看-日韩精品一区二区三区在线视频| 久久99国产欧美精品-深夜宅男宅女在线观看-骚虎三级在线免费播放-精品国模人妻视频网站| 中文国产成人精品久久一-亚洲一区二区精品视频网站-在线深夜羞羞福利视频-麻豆视频传媒免费入口| 国产 av 一区二区三区-日韩黄色三级三级三级-久久精品视频这里只有精品-日韩精品中文字幕亚洲| 一区二区在线观看黑人-久久久精品人妻一区二区三区综合-成人内射国产免费观看-四虎在线免费视频观看| 少妇人妻上班偷人露脸-欧美中文字幕乱码视频-欧美韩日本一本交道免费-国产一区,二区,三区免费视频| 未满十八禁止免费观看网站-国产夫妻福利在线观看-亚洲国产黄色精品在线-日韩亚洲一卡二卡三卡| 福利一区福利二区刺激-亚洲精品久久麻豆蜜桃-久久av蜜臀人妻一区二区三区-国产av剧情精品播放网站| 中文字幕久久精品一区二区三区-99国产麻豆精品人人爱-91麻豆精品福利视频-国产精品亚洲一区中文字幕| 91亚洲综合成人在线-久久精品亚洲av少妇-日本av一区在线视频-9国产精品久久久久麻豆| 亚洲av色香一区二区三含羞草-av毛片在线观看网站-中文字幕一区二区人妻中文字-91精品人妻日韩一区二区| 亚洲精品一区二区三区探花-av在线免费播放成人-精品亚洲一区二区三区在线播放-国产精品午夜福利亚洲综合网| 亚洲国产精品无吗一区二区-伊人久久综合在线观看-欧美日韩在线精品视频二区-国产精品一区二区国产主播| 亚洲中文字幕中出在线-美女口爆吞精在线播放-亚洲欧美清纯唯美另类-国产一区二区三区免费观看不卡| 国产精品视频午夜福利-一本大道久久综合一区-成年深夜福利在线观看-国产传媒免费在线视频| 久久精品国产久精国产爱-久久超碰97中文字幕-久热这里只有精品视频一区-日韩av在线免费观看| 国产人妖直男在线视频-午夜福利视频合集91-亚洲五月自拍欧美第一页-国产主播免费在线一区二区| 深夜福利在线观看日韩-国产成人夜色高潮在线观看-熟女人妻少妇精品视频-97在线观看完整免费| 日本在线有码中文视频-精品亚洲综合一区二区三区-国产午夜福利一级二级三级-天堂三级成人久久av| 高清国产av一二三四-少妇激情高潮视频网站-被公么玩弄邻居人妻中文字幕-亚洲免费成人av在线| 精品人妻在线一区二区三区-国内av在线免费观看-亚洲av影片一区二区三区-久久精品女同亚洲女同13| 国产精品日本一区二区不卡视频-尤物在线视频免费观看-中文字幕精品高清中国-最新精品国产自偷在自线| 亚洲欧美日韩不卡视频-四虎永久在线精品免费看-久久av丰满熟妇极品-亚洲国产精品中文字幕一区| 国产精品自在线拍国产-久久精品韩国日韩精品-久久夜色国产精品亚洲av蜜桃-日韩精品一区二区三区四区免费| 日本成熟人妻在线看片-亚洲国语精品激情在线-欧美性生活之欧美日韩-成人黄色av在线观看| 日韩精品中文一区二区三区在线-午夜视频国产在线观看-日韩中文字幕av有码-最新日韩精品视频免费在线观看| 亚洲乱码中文字幕综合-欧美日韩亚洲综合久久精品-美女隐私无遮挡免费网站-国产精品激情av在线播放| 免费十八禁一区二区三区-国产精品一区二区三区99-在线一区二区三区男男视频观看-精品欧美一区二区三区人妖| 国内精品国产三级国产-91制片厂麻豆果冻剧情观看-日韩中文字幕有码在线视频-精品人妻伦一区二区三区久久| 久久噜噜噜精品国产亚洲综合-91精品国产高清久久福利-精品国产一区二区三区麻豆-日本加勒比一区二区在线观看免费| 免费观看国产裸体视频-久久亚洲精精品中文字幕早川悠里-99精品国产一区二区青青牛奶-久久精品成人av免费观看| 亚洲老妈激情一区二区三区-夜晚福利视频亚洲精品自拍视频-亚洲av永久精品一区二区在线-中文国产人精品久久蜜桃| 国产成人自拍视频精品-丝袜美腿亚洲一区二区刘亦菲-91精选国产在线视频-欧洲美熟女乱又伦免费| 特大毛片毛片免费视频-成人伊人青草久久综合网-91亚洲蜜桃内射后入在线观看-日韩情色电影中文字幕| 久久中文字幕人妻淑女-日韩欧美亚洲一中文字幕-日本免费一区二区三区视频-亚洲精品乱码免费精品乱码| av网站在线观看华人免费-美女露下体让人舔视频网站-六月丁香激情综合爱爱-宅福利有番号亚洲麻豆91| 91老熟女老女人国产老太-av在线亚洲av男人的天堂-国产精品久久久区三区天天噜-能看不卡视频网站在线|