色呦呦网址在线观看,久久久久久久久福利精品,国产欧美1区2区3区,国产日韩av一区二区在线

When WC grains in cemented carbide are less than 0.5 μ m, the finer the grains are, the fewer the defects are, and the higher the bending strength and hardness are The particle size of WC powder used to produce ultrafine cemented carbide is much smaller than that of WC powder used in general cemented carbide. The WC powder has high activity and is easy to cause grain growth in the sintering process, which is one of the crack sources.

At present, there are two main methods to control the grain size:

First, a new sintering process is adopted. The results show that the densification of dozens of nano WC Co composite powders can be completed after sintering at 1400 ℃ for 30s, and the grain size is 0.2 μ m, but if the sintering time is extended to 60s, the grain size will grow rapidly to 2.0 μ M. The new sintering processes that can be used for nano WC Co cemented carbide composite powder mainly include microwave sintering, hot isostatic pressing sintering, discharge plasma sintering and two-stage sintering.

Second, adding inhibitors of grain growth to inhibit grain growth, VC, TAC and Cr3C2 are often used inhibitors.

In this paper, the inhibition mechanism, the factors affecting the effect of inhibitors, the way of adding inhibitors, the commonly used inhibitors, the development of the latest inhibitors and the influence of inhibitors on the comprehensive properties of alloys are introduced.

Application of Grain Growth Inhibitors in Cemented Carbide 2

Inhibition mechanism and influencing factors of inhibitors

The driving force for the grain growth of cemented carbide comes from the reduction of surface energy. The grain growth of WC is mainly through the dissolution precipitation mechanism of WC, that is, small grain WC dissolves in the liquid phase and precipitates on the surface of large grain WC. For WC Co cemented carbides, the coarsening of WC grains can be limited by the addition of grain growth inhibitors.  

The addition of inhibitors slows down the dissolution precipitation rate of WC, and there are three inhibition mechanisms:

1. The inhibitor adsorbs on the surface of carbide particles, which reduces the surface energy of WC and the solubility of WC in liquid phase.

2. The inhibitor dissolves in liquid CO, which slows down the growth of WC through liquid recrystallization.

3. The migration of WC interface was hindered by the segregation of inhibitors along WC / WC interface, which prevented the aggregation and growth of WC particles.

The inhibition effect of inhibitors is determined by the following factors:

1. Decreasing the particle size of WC powder increases the grain boundary area of WC Co. inhibitors can be widely distributed on the surface of WC, but they can not be increased indefinitely. Their limit value depends on their saturation concentration in the bonding phase.

2. Cobalt content. With low content of binder and short free stroke, the inhibitor is easy to play its role at a certain temperature.

3. Uniformity of powder mixing. The uneven distribution of the binder phase in the mixed powder will lead to the difference of the effect area of inhibitors on WC grain growth in the sintering process; the uneven distribution or large size of the inhibitors in the mixed powder will lengthen the diffusion route required by the inhibitors

4. Alloy sintering temperature. With the increase of sintering temperature, the amount of liquid phase and the content of grain growth inhibitor need to be increased in order to keep the high concentration of inhibitor in the liquid phase Therefore, the smaller the powder size, the lower the cobalt content, the more uniform the powder mixing and the lower the sintering temperature are, the better the inhibition effect of the inhibitor is.

Application of Grain Growth Inhibitors in Cemented Carbide 3

Adding ways of grain growth inhibitor

Inhibitors are mainly added in three ways:

1. WC, CO and grain growth inhibitor were mixed in the wet grinding process.

2. Before w carbonization, oxide corresponding to grain growth inhibitor was mixed.

3. The third method is to wet mix the salt solution of the inhibitor with blue tungsten or yellow tungsten, and form coating powder with blue tungsten or yellow tungsten before reduction, and then conduct further thermal decomposition and reduction.

Zastosowanie inhibitorów wzrostu ziarna w w?gliku spiekanym 4

Types of grain growth inhibitors

Transition metal carbides

Transition metal carbides are common inhibitors of grain growth. The effectiveness of transition metal carbides in inhibiting WC grains is related to their own thermodynamic stability. The order of their thermodynamic stability is VC > Cr3C2 > NBC > TAC > tic > ZrC > HFC. However, each kind of carbide has a maximum amount that can be added, which has no further effect on inhibiting the growth of WC grains. At a certain temperature, the amount of carbide additives depends on the saturation concentration of the carbide in the binder phase and the content of the binder phase Table 2 shows the solubility of various additives in CO phase. It can be seen from the table that VC and Cr3C2 have the highest solubility in CO phase and they have the lowest binary eutectic temperature, so they are widely used as WC Co grain growth inhibitors.

Application of Grain Growth Inhibitors in Cemented Carbide 5

Rare earth element

Rare earth element is one of the common additives, which can inhibit the grain growth, improve the structure distribution, purify the grain boundary, and play an effective role in strengthening and toughening the cemented carbide. At the same time, rare earth can also reduce the sintering temperature of cemented carbide, which can solve the contradiction between controlling grain growth and Sintering Densification. the increase of the macro compressive stress on the alloy surface is also an important reason for the increase of the strength of WC Co cemented carbide by the addition of rare earth oxides.

Boron and phosphorus

It is found that the sintering temperature of the cemented carbide with boron can be reduced to 1340 ℃, with the decrease of sintering temperature, the micro grains of the alloy are obviously refined, which is conducive to the improvement of the alloy performance, and the addition of boron has little effect on the wettability of the bonding phase and WC phase, and the bending strength of the alloy is not affected. The sintering temperature of WC Co can be reduced to 1050-1100 ℃ by adding a small amount of Ni and P powder. The mechanism is that the eutectic temperature of Ni-P is far lower than the melting point of Co. after adding Ni and P, the liquid phase can appear at a lower temperature, which makes the dissolution and precipitation of solid particles and the formation of framework occur in advance, and the sintering process is more sufficient, thus inhibiting the growth of WC grains.

Copper molybdenum metal inhibitor

The addition of a small amount of Cu to wc-13fe / Co / Ni cemented carbide can refine the spheroidized WC grains. This is mainly because Cu will dissolve into the Fe / Co / Ni binder during the sintering process, reducing the solubility of WC in the binder, thus reducing the rate of grain growth during the dissolution re precipitation process. And copper also spheroidizes WC grains. In the sintering process of cemented carbide, molybdenum is coated around the cemented phase, which improves the wettability between the cemented phase and the cemented phase, so as to refine the particles of cemented phase

Effect of grain growth inhibitor on properties of alloy

The effect of grain growth inhibitors on the properties of the alloy is mainly reflected in the hardness and bending strength of the alloy Different additives have different mechanisms of inhibiting grain size, so different inhibitors of grain growth have different effects on properties.

Transition metal carbides

The addition of VC, Cr 3C 2 and other additives can effectively improve the heat resistance and wear resistance of WC Co cemented carbide. Moreover, the high temperature strength and high temperature hardness of the alloy can be effectively improved when the additive is appropriate, but the room temperature strength of the alloy can be reduced and the alloy becomes brittle. Therefore, the amount of additives must be controlled within a certain range For example, for WC-6% CO and WC-10% Co alloys, the addition of cr2c3 reduced the room temperature bending strength of the alloy. When the content of Cr 2C 3 is 0.3% ~ 0.5% (mass fraction of CO content), the room temperature bending strength of the high Co alloy will not be affected obviously, but for the low Co alloy, the room temperature bending strength will be decreased obviously. Adding TAC and NBC will result in the same result The effect of VC on the microstructure and properties of wc-6.5% Co cemented carbides was found. It was found that VC inhibited the growth of WC grains, which resulted in obvious grain refinement and narrowed the distribution of grain size. The grain size decreased from 0.5-1 μ m without adding VC to 0.15 μ m with adding 2.0% VC. At the same time, the hardness of the alloy is greatly improved by adding VC, and the maximum value is 94.1 HRA when VC content is 2.0%. But it also reduces the strength of the alloy When VC content is 0.5%, the hardness and toughness of the alloy are 93.0hra and 11.2MPa · M 1 / 2, and the comprehensive properties are the highest. The addition of TAC can not only prevent the WC grains from growing too much, but also reduce the carbon content of the alloy

Rare earth element

The hardness of WC-20 (Fe / Co / Ni) alloy increased with the increase of rare earth content. The addition of rare earth can improve the properties of w-co-ti alloy, especially improve the impact resistance of Shejin. At the same time, rare earth can inhibit the grain aggregation and growth of (Ti, w) C solid solution and refine the grain.  When rare earth oxide is added to WC Ni alloy, the strength of bonding phase Ni increases due to dispersion strengthening of rare earth oxide. When the rare earth content is 1.2% ~ 1.6% of bonding metal content, the bending strength of the alloy reaches the maximum value (1680mpa when CeO 2 is added, 1900mpa when Y2O3 is added). The bending strength of WC-8% Co alloy is increased to a certain extent by adding 0.25% ~ 1.00% of the mixed rare earth oxide, and it can be increased by 11.5% when adding 0.25% ~ 0.50% of the rare earth oxide, but the excessive addition of rare earth will lead to the decrease of the bending strength. Therefore, the bending strength of cemented carbide with rare earth elements can be greatly improved.

Cu&Mo metal inhibitors

Adding a small amount of copper into the cemented carbide can not only improve the strength of the alloy, but also improve the impact toughness of the alloy.

When a small amount of copper is added to WC-13% Fe / Co / Ni, the hardness of the alloy decreases, while the bending strength increases greatly. When the amount of copper is about 0.8%, the bending strength and hardness of the alloy are 2370 MPa and hra84.4 respectively. See Table 3 below. When Mo was added to WC Co, the bending strength and India increased with the increase of Mo addition. The bending strength reached the maximum value when Mo addition was 5%, and reached the peak value of 19.25gpa when Mo addition was 7.5%. However, when the amount of Mo is more than 5%, the bending strength decreases gradually, which is due to the embrittlement of the sample caused by the presence of intermetallic compound CO3(Mo, w)3C.

Application of Grain Growth Inhibitors in Cemented Carbide 6

国产高清三级自拍视频-最近日本免费播放视频午夜-日本女优一级片中文字幕-在线播放深夜精品三级| 日日夜夜久久国产精品-国产男女无遮挡猛烈免费观看-在线观看热久精品视频-国产香蕉视频在线内射| 中国美女欧美熟妇视频-五月爱婷婷丁香六月色-国产特黄特色成年女人毛片免-人妻精品一区二区三区久久| 蜜桃臀欧美日韩国产精品-最近欧美日韩一区二区-亚洲综合成人一区二区三区-免费五十路熟妇在线视频| 美女脱内衣内裤露出咪咪-美女一区二区三区免费观看-国产网红女主播在线视频-久久亚洲春色中文字幕| 换脸av一区二区三区-少妇精品亚洲一区二区成人-亚洲熟女综合一区二区三区-国产91久久精品成人看| 欧美日本国产一区二区三区-亚洲精品成人午夜在线观看-国产精品一二三在线看-国产成人传媒在线播放| 少妇特殊按摩高潮连连-国产成熟美女三级视频-亚洲男人天堂成人免费-国产粉嫩美女在线观看| 91精品在线播放黑丝后入-97免费在线播放视频-av网站天堂网国产av-亚洲熟妇乱色一区二区三区| 国产福利一区二区写真-久久国产电影在线观看-亚洲国产一区二区三区亚瑟-中文字幕乱码亚洲无线码二区| 日韩精品成人一区二区三区-亚洲综合中文字幕第一页-久久伊人亚洲中文字幕-花季传媒视频无限制观看| 特大毛片毛片免费视频-成人伊人青草久久综合网-91亚洲蜜桃内射后入在线观看-日韩情色电影中文字幕| 亚洲不卡福利在线视频-亚洲一级特大黄色小视频-日本久久一级二级三级-国产精品剧情av在线观看| 日韩人妻毛片中文字幕-国产精品亚洲综合第一页-国产精品久久亚洲av-亚洲国产精品一区二区不卡| 日韩熟女人妻中文字幕-亚洲视频自拍偷拍免费-91国内精品久久精品一本-日韩高清一区二区不卡视频| 色激情五月关键词挖掘-日本精品一区二区三区视频-亚洲精品一区二区三区四区久久-亚洲综合久久激情久久| 久久精品国产亚洲av五区-日韩麻豆视频在线观看-亚洲欧洲国产成人综合在线-美利坚合众国亚洲视频| 国产大奶子在线播放免费-中文字幕在线观看精品亚洲-日韩欧美精品一区二区三-国产手机av免费在线观看| 久久精品熟女亚洲av麻豆-国产精品久久99粉嫩-校园春色另类综合在线视频-久久亚洲精品国产日韩| 狠狠操夜夜操天天干天天-午夜一级视频在线免费观看-我要看欧美一级黄色录像-91嫩草国产亚洲精品| 天天躁夜夜躁狠狠85麻豆-操美女逼视频免费软件-国产精品一区二区在线观看-一区二区三区免费观看视频在线| 人妻精品一区二区视频免费-99热视频免费在线观看-亚洲av第一第二第三-乱码人妻精品一区二区三区| 九九久久精品国产婷婷-亚洲少妇视频在线观看-国产网友精品自拍视频-超碰在线成人免费精品| 日韩精品一区二区三中文字幕-欧美亚洲日本精品一区二区-日韩av亚洲在线观看-亚洲欧美国产日韩激情| 拉风色国产精品一区二区三区-av一级不卡手机在线观看-亚洲欧美日韩国产色另类-青青草伊人视频在线观看| 青青草视频成人在线公开-激情中文字幕一区二区三区-亚洲国产精品综合久久网各-日本中文字幕有码高清| 一本久道视频无线视频试看-亚洲国产精品一区二区三区久久-中文字幕色偷偷人妻久久-久久精品99国产精品中| 亚洲天堂成人av影院-日韩精品国产一区在线久草-欧美国产另类久久久精品-91午夜精品久久香蕉| av福利在线播放网站-午夜福利在线观看精品-久久精品女人av天堂-日本中文字幕在线乱码| 久久久免费福利视频观看-成年人在线观看视频免费播放-噜噜中文字幕一区二区三区-视频一区视频二区三区| 亚洲精品在线观看一区二区三区-亚洲高清在线自拍视频-日本一区二区三区午夜视频-日韩精品极品视频在线| 日日夜夜久久国产精品-国产男女无遮挡猛烈免费观看-在线观看热久精品视频-国产香蕉视频在线内射| 美女脱掉内裤露屁屁最新章节-成人中文字幕在线观看的-国产极品尤物粉嫩在线观看-在线视频一区二区中文字幕| 日本岛国三级黄色录像-日韩久久成人免费电影-中文字幕日韩专区一区二区-国产成人大片在线播放| 国产一区二区精品在线播放-亚洲欧美精品伊人久久-亚洲精品日韩在线播放-国产精品色av一区二区三区| 久久夜色国产精品亚洲-国产视频一区二区三区免费观看-亚洲一区二区成人在线观看-日韩精品一区二区三区在线视频| 国产亚洲一区二区三区综合片-亚洲天堂日韩精品在线-有码视频在线观看日本专区-亚洲精品成人福利在线| 十八禁黄网站免费观看在线-欧美日韩精品久久久免-黄色av免费在线观看网站-国产在线高清一区二区三区av| 久久夜色国产精品亚洲-国产视频一区二区三区免费观看-亚洲一区二区成人在线观看-日韩精品一区二区三区在线视频| 超碰成人av免费观看-伊人色综合久久天天伊人婷-av天堂激情在线观看-国产精品自拍国产精品| 成人精品一区二区三区不卡-十八禁啪啪啪一区二区三区-后入黑丝美女在线观看-国产熟女啪啪免费视频|