Austenitic stainless steel has good corrosion resistance because of its high chromium content and dense oxide film. When Cr18% and Ni8% are contained, a single austenite structure can be obtained. Therefore, austenitic stainless steel has good corrosion resistance, plasticity, high temperature performance and welding performance. However, under different working conditions, austenitic stainless steel welding joints often face some special problems, which are easy to cause construction defects such as intergranular corrosion, stress corrosion, knife corrosion, welding hot cracks, α phase embrittlement and so on.

Corrosion analysis of welded joints

Intergranular corrosion of welded joints

Intergranular corrosion is one of the most important corrosion problems of austenitic stainless steel. Once intergranular corrosion occurs, its strength will almost lose when it is serious, and intergranular fracture will occur when a certain stress is applied. The intergranular corrosion of austenitic stainless steel welding joint is mainly caused by chromium carbide precipitation. When the austenitic stainless steel is sensitized in the temperature range of 500 ~ 800 ℃, the diffusion rate of supersaturated solid solution carbon to the intergranular boundary is faster than that of chromium, and the carbon in supersaturated solid solution is combined with chromium near the grain boundary, When the chromium content in the region is reduced to below the limit content (w (CR) 12.5%) required for passivation, the corrosion of the region will be accelerated and intergranular corrosion will be formed. The results show that the intergranular corrosion in the sensitized temperature zone of HAZ occurs in the region where the peak heating temperature is between 600 ℃ and 1000 ℃. The reason for intergranular corrosion is still the precipitation of chromium carbide at austenite grain boundary. The main preventive measures to reduce and prevent intergranular corrosion include:

① Small specification (small current, high welding speed) and multi pass welding are adopted;

② The carbon content in the base metal and welding material should be reduced as much as possible, and the welding material with C content less than 0.03% should be used;

③ As a result, Cr diffuses to the grain boundary more quickly in ferrite than in austenite, which reduces the phenomenon of poor chromium in austenite grain boundary;

④ The addition of Ti, Nb and other elements with stronger affinity to carbon than chromium in steel and welding materials can form stable compounds with carbon bonding, thus avoiding chromium depletion at austenite grain boundaries.

Stress corrosion of welded joints

The stress corrosion cracking of stainless steel is the most harmful corrosion behavior. There is no deformation when cracking. The accident is often sudden and the consequences are serious. There are many factors influencing the stress corrosion cracking of stainless steel under service conditions, including the composition, structure and state of the steel, the type of medium, temperature, concentration, stress properties, size and structural characteristics.

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 2

The main measures to reduce and prevent stress corrosion are as follows:

① Avoid strong assembly, mechanical impact and arc burn, reduce cold work deformation and stress;

② Strictly control impurities in media and environment (especially chloride, fluoride, etc.);

③ Reasonable material selection (base metal, welding material): avoid grain coarsening and hardening martensite structure;

④ The weld is well formed without any stress concentration (such as undercut);

⑤ Arrange welding sequence reasonably to reduce stress;

⑥ Anti corrosion treatment: add corrosion inhibitor to coating, lining or cathodic protection.

 

Hot crack sensitivity analysis of welded joints

The hot cracks of austenitic stainless steel are mainly crystalline cracks, which are produced during the solidification process of liquid metal of weld metal. At this time, primary crystals exist in eutectic melting point, mainly between dendrites. The main reasons are as follows:

① S, P, C and so on form low melting point eutectic with Ni (for example, the melting point of NIS + Ni is 644 ℃), which weakens the grain boundary strength;

② Austenitic stainless steel has the advantages of large distance between liquidus and solidus, long crystallization time, strong dendrite orientation and easy to produce segregation of impurity elements;

③ The thermal conductivity of steel is small, and the linear expansion coefficient is large, so it is easy to produce stress.

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 3

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 4 

The main measures to prevent welding hot cracks include:

① The contents of harmful impurities sulfur and phosphorus in base metal and welding material shall be strictly controlled;

② About 5% ferrite is produced in the weld, which disturbs the direction of austenite columnar crystal;

③ Small current and fast welding process are adopted.

Control of ferrite content in welded joints

The content of ferrite in weld metal of austenitic steel is not only related to the formation and thermal strength of α (σ) phase embrittlement, but also directly affects the hot cracking resistance of joint. The longer the heating time, the longer the high temperature residence time, the more precipitation, which will seriously affect the mechanical properties of the joint. From the point of view of hot cracking resistance, a certain amount of ferrite is required in the weld metal. However, considering the α phase embrittlement and thermal strength, the lower the ferrite content is, the better. Therefore, the content of ferrite must be strictly controlled for high temperature strength welded joints. In some cases, austenitic weld metal must be used.

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 5

青青草视频成人在线公开-激情中文字幕一区二区三区-亚洲国产精品综合久久网各-日本中文字幕有码高清| 少妇人妻上班偷人露脸-欧美中文字幕乱码视频-欧美韩日本一本交道免费-国产一区,二区,三区免费视频| 国产亚洲成人精品久久久-亚洲免费av高清在线观看-在线观看国内自拍视频-亚洲国产成人精品综合色| 国产精品日本一区二区不卡视频-尤物在线视频免费观看-中文字幕精品高清中国-最新精品国产自偷在自线| 青青成年人性生活视频-日韩精品成人亚洲天堂-久久永久免费人妻精品我不卡-成人国产精品三上悠亚久久| 国产一区二区在线中文字幕-欧洲中文字幕国产精品-国产精品蜜臀av免费观看四虎-国产一级特黄99久久| 97中文字幕一区二区三区-国产精品亚洲av无人-亚洲国产精品自产拍久久-成人深夜福利在线视频| 人妻少妇中文字幕久久精品-水蜜桃av一区二区三区在线观看-日韩熟女精品一区二区三区-久久国产综合激情对白| 少妇被无套内谢免费视频看看-不卡中文在线观看网站-国产精品男女爽免费视频-91精品福利视频久久| 亚洲国产成人精品毛片九色-成年片黄色大片品赏网-亚洲男人天堂色噜噜av-人妻免费精品久久一区| 国内精品欧美久久精品-国产极品尤物美在线观看-日本经典视频一区二区三区在线-国模91九色精品二三四| 亚洲免费中文字幕一区二区三区-超碰在线免费在线免费-国产熟女茂密的黑森林-色姑娘久久综合网天天| 中美高清在线观看av-精品视频中文字幕天码-日韩高清一二三区在线观看-精品人妻91一区二区三区| 蜜桃臀欧美日韩国产精品-最近欧美日韩一区二区-亚洲综合成人一区二区三区-免费五十路熟妇在线视频| 亚洲精品人妻中文在线-国产成人精品视频三级-麻豆视频黄片在线免费观看-亚洲性色精品一区二区在线| 午夜福利国产在线播放-中文字幕日产乱码久久正宗-亚洲精品成人久久69-99精品国产免费久久| 国内国产精品国产三级-美女性爽潮喷白丝小仙女-国产精品自拍露脸在线-国产精品亚洲综合日韩| 亚洲一区二区三区视频观看-日韩精品一二三四区视频-亚洲码与欧洲码区别入口-日韩精品大片一区二区三区| 精品国产亚洲av蜜臀-欧美亚洲伦理在线视频-久久亚洲国产成人影院av-国产精品99蜜臀久久不卡二区| 国产激情在线观看视频-久久久精品国产视频在线-亚洲国产成人精品在线-亚洲乱码国产乱码精品视频| 日韩成人大片一区二区三区-国产一级淫片av免费-18禁免费观看网站入口-国产黄色特级片一区二区三区| 免费十八禁一区二区三区-国产精品一区二区三区99-在线一区二区三区男男视频观看-精品欧美一区二区三区人妖| 亚洲天堂久久中文字幕-高清国产一级片免费看-伊人狼人综合日日夜夜-手机看片高清国产日韩| 熟妇女人妻丰满少妇中文-最新国产成人在线网站-亚洲性日韩精品一区二区三区-亚洲免费熟女做爰视频| 久久亚洲av综合悠悠色-91手机精品免费在线播放-午夜福利一区二区三区在线播放-97在线精品观看视频| 日韩精品成人一区二区三区-亚洲综合中文字幕第一页-久久伊人亚洲中文字幕-花季传媒视频无限制观看| 日韩熟女av在线观看-中文字幕人妻丝祙乱一区三区-亚洲国产精品第一区二区三区-欧美制服丝袜一区二区三区| 青青草免费视频手机版-男人天堂欧美日韩在线-成人黄色av在线免费看-超短裙女教师在线观看| 国产精品内射在线免费看-99久久国产精品一区二区三区-久久国产精品午夜福利-亚洲av精品一区二区三区| 亚洲永久精品在线观看-成人av在线观看免费-蜜臀av免费一区二区三区-成人av在线久色播放| 少妇裸淫交视频免费看-欧美日韩中文字幕第一页-91精品看黄网站在线观看-国产精品一区二区三区色噜噜| 亚洲中文字幕高清乱码毛片-国产成人午夜福利精品-久久毛片绝黄免费观看-国产亚洲成性色av人片在线观| 日韩精品人妻久久久一二三-亚洲精品呻吟久久粉嫩av-女同按摩高潮中出亚洲-亚洲成人精品福利在线| 国产免费无套精品视频-日本特色特黄aaa大片免费-日本精品免费一区二区三区-九九热精品视频在线免费| 国产韩国精品一区二区三区-久久精品人妻一区二区三区av-黄片视频在线观看欧美-国产成人自拍在线视频| 久久国产精品亚洲va麻豆-嫩模大尺度偷拍在线视频-免费三级在线观看自拍-天堂av在线男女av| 在线免费观看四虎黄色av-亚洲成人av高清在线-成人性生交大片免费在线-四虎成人精品在线观看| 国产av蜜臀一区二区三区野战-欧美精品久久精品推荐-亚洲有吗黄色日韩视频-中文字幕在线乱码人妻| 九九热在线视频精品一-国产乱码精品一区二区蜜臀-乱妇乱熟女妇熟女网站视频-国产精品午夜视频在线| 国精品视频在线播放不卡-日韩av免费观看在线-亚洲这里只有精品在线观看-免费的精品一区二区三区| 在线观看日韩不卡视频-深夜福利成人羞羞免费视频-日韩欧美精品综合另类-黄色特级一级片中文字幕|