Hey everybody, a new material weekly on surface grinding of ultra-fine cemented carbides. Reading this probably cost you about 15 minutes

Abstract of this article: The grinding experiment of superfine cemented carbide was carried out on a plane grinder with diamond grinding wheel. The grinding surface morphology was observed by scanning electron microscopy and the surface roughness was measured by surface roughness tester. The influence of grinding parameters on the surface roughness of ultra-fine cemented carbide grinding was analyzed. The results show that the grinding surface roughness of superfine cemented carbide increases with the increase of grinding wheel size at the same cutting depth. When grinding with the same grain size grinding wheel, the surface roughness of ultra-fine cemented carbide grinding increases with the increase of the cutting depth. When the cutting depth increases to a certain value, the surface roughness decreases gradually.

Introduction

WC-Co cemented carbide is a conventional tool material. In recent years, with the continuous development of cutting technology, the requirements for the strength, hardness and wear resistance of tool materials are getting higher and higher. Compared with traditional structural cemented carbides, superfine cemented carbides (WC grain size 0.1-0.6 um) have higher strength, hardness and wear resistance, so they are widely used in tool manufacturing industry.

grinding parameters

Grinding with a diamond grinding wheel is the main method to produce cemented carbide tools. Many studies have shown that grinding surface roughness has an important influence on the cutting performance and service life of cemented carbide tools. Up to now, the grinding research of cemented carbide at home and abroad mostly focuses on the improvement of traditional structure cemented carbide grinding process and surface quality control, while the grinding process of superfine cemented carbide, especially the grinding surface roughness, is rarely studied. Therefore, through grinding experiments, the influence of grinding wheel size and cutting depth on surface roughness of ultra-fine cemented carbide grinding is discussed by means of scanning electron microscopy (SEM) and surface roughness tester, in order to provide the basis for the optimization of grinding process of ultra-fine cemented carbide.

Test materials and methods

Test materials

The test material is ultra-fine grain WC-Co cemented carbide sintered by HIP technology. The sample size is 10 mm x 10 mm x 10 mm. The chemical composition and mechanical properties are shown in Table 1.

Table 1 Chemical composition and mechanical properties of test materials

grinding parameters

The samples were clamped with precision flat clamp and ground on the surface grinder Model M7120. The grinding wheel used is resin bonded diamond flat grinding wheel with an outer diameter of 250 mm, a width of 25 mm and a diamond layer thickness of 8 mm. The coolant is a mixture of water and emulsified oil. The experimental grinding parameters are shown in Table 2.

grinding parameters

After grinding test, samples were cleaned with anhydrous acetone in the ultrasonic cleaner for 30 minutes and dried by hot air. Scanning electron microscopy with back reflection detector was used to observe the grinding surface morphology of the sample. The grinding surface roughness of the sample was measured along the direction perpendicular to the grinding direction with the surface roughness tester. The sampling step was 0.25 mm, and the evaluation length was 4 times of the step. Each sample was measured six times and the results were averaged.

test result

Fig. 1 shows the variation of grinding surface roughness with grinding wheel size under the same cutting depth (ap=10 um). It can be seen from the graph that the grinding surface roughness increases with the increase of grinding wheel size at the same cutting depth. But the influence of grinding wheel particle size on surface roughness is different. Compared with 150 # grinding wheel, using 280 # grinding wheel, the change of surface roughness is smaller while using W20 grinding wheel, the change of surface roughness is larger. Figure 2 shows the variation of surface roughness with the depth of cut AP when grinding with the same grinding wheel (150 #). It can be seen from the graph that the roughness of the grinding surface increases approximately linearly with the increase of AP when AP is less than 15 micron. But when AP > 15 um, the grinding surface roughness decreases gradually with the increase of shear depth, which is obviously different from the grinding test results of traditional structure cemented carbide.

grinding parameters

Surface roughness is the direct reflection of grinding surface morphology. In order to analyze the causes of the above parameters affecting the grinding surface roughness of ultra-fine cemented carbide, the surface morphology of grinding samples was observed by SEM with back reflection electron detector. Figure 3 shows the back-reflection electronic image of the grinding surface morphology of the sample ground with different diamond grinding wheels under the same cutting depth. As can be seen from the figure, the grinding marks on the surface of superfine cemented carbide ground by W20 grinding wheel are narrow and shallow, the bottom and sides are smooth, and the uplifts on both sides are very small (see Figure 3a). After grinding with 280 # grinding wheel, cracks appear on the grinding surface. The grinding marks are wide and deep, and the bottom and sides are rough with scaly fracture structure (see Fig. 3b). After grinding with 150 # grinding wheel, although the depth of grinding marks on the grinding surface is relatively shallow, there are more grinding debris and fracture structure (see Figure 3c), showing obvious brittle fracture characteristics.

Analysis and discussion

Grinding is accomplished by a large number of high hardness Abrasives arranged randomly on the surface of the grinding wheel. Each abrasive grain can be regarded as a tiny cutter approximately. The grinding surface is formed by the relative motion of these numerous irregular cutting micro-edges on the surface of the ground material. Therefore, the grinding wheel size, cutting depth and mechanical properties of the ground material will inevitably affect the grinding surface morphology, and then affect the grinding surface roughness.

Before the test, the sharp diamond abrasives can be simplified into cones because the same dressing method and material are used for each wheel. At the same time, due to the high stiffness of grinding machine system and the cooling effect of grinding fluid, the thermal deformation of diamond grinding wheel in contact with the sample during grinding can be neglected, and the actual cutting depth can be replaced by the set cutting depth of the grinding wheel. Then, in the process of plane grinding, the radial grinding force Fp exerted by grinding wheel and the maximum cutting thickness Hm of a single abrasive grain can be obtained by formula (1) and formula (2), respectively.

grinding parameters

In the formula, CF is a constant related to the type of material being ground; Vw is the speed of workpiece, m/min; Vc is the speed of grinding wheel, m/s; B is the width of grinding, mm; theta is the half-angle of cone top of abrasive grain; AP is the set cutting depth, micron; FA is the axial feed, mm; m is the effective number of abrasive grains per unit area of grinding wheel. D is grinding wheel diameter, mm.

The removal mechanism of hard and brittle materials such as cemented carbide and ceramics usually includes inelastic deformation removal, brittle removal, and material powdering, etc. It depends on the force condition of grinding surface during grinding. When the normal load on the surface of the ground material below the abrasive grain is lower than the critical value of cracks in the material, the ground material is removed by non-elastic deformation such as sliding, plowing and chip formation. When the normal load on the grinding surface exceeds the critical normal load on which the material cracks occur, the grinding cracks nucleate and gradually extend to the grinding surface, and the material is removed by brittle means such as peeling and fragmentation. The harder phase in the material will be powdered under larger normal load. The low hardness bonding phase will be coated on the surface of the powdered hard phase and partially removed with the hard phase debris.

In the grinding process of cemented carbide, the critical normal load produced by cracks and debris can be expressed as

grinding parameters

In the formula, lambda is a comprehensive constant, lambda_2*105; H is the hardness of the material; Kc is the fracture toughness. Formula (1) shows that under the same grinding conditions as wheel speed, workpiece speed, grinding width and axial feed, the normal grinding force Fp on the surface of the ground material is proportional to the cutting depth and increases linearly with the increase of ap; Formula (2) shows that the maximum cutting of a single abrasive particle is achieved. The thickness increases with the increase of AP and decreases with the increase of effective abrasive number M.

In this experiment, under the same cutting depth (i.e. the same Fp), the normal loads exerted by a single abrasive on the surface of the ground material are also different due to the different particle size of the diamond grinding wheel. Due to a large number of effective abrasives, the normal load exerted by a single abrasive on the grinding surface is small. Therefore, when superfine cemented carbide is ground by W20 grinding wheel, its removal mode is mainly inelastic deformation. At the same time, due to a large number of effective abrasives, the maximum cutting thickness Hm of a single abrasive is relatively small, and only slight friction and plowing occur on the grinding surface, so the grinding surface has narrow and shallow grinding marks, smaller uplift (see Fig. 3a), and lower surface roughness. With the increase of grinding wheel size, the number of effective abrasives decreases, and the normal load exerted by a single abrasive on the grinding surface increases. When the load is larger than the critical normal load of the crack-fragment of superfine cemented carbide material, cracks and cracks begin to appear on the grinding surface (see Fig. 3b). With the increase of grinding wheel size, the degree of cracking becomes more serious (see Fig. 3c). The main way of material removal is brittle removal. Compared with slip friction and slight plow, cracks and cracks seriously deteriorate the roughness of grinding surface, which is reflected in the measurement value of surface roughness. The roughness of grinding surface decreases with the increase of grinding wheel size (see Fig. 1). It is precise because of the difference of material removal methods that the surface roughness of grinding surface varies greatly when grinding with W20 grinding wheel.

When grinding with the same grinding wheel and different cutting depth, the normal grinding force Fp of the grinding wheel increases with the increase of the cutting depth, and the normal load on the grinding surface increases with the increase of the single grinding particle, which makes the material removal mode of the grinding surface of ultra-fine cemented carbide change. When the cutting depth AP is less than 5 micron, the normal load exerted by a single abrasive particle on the grinding surface is small. The material removal mode during grinding is mainly plowing in inelastic deformation, which produces deep grinding marks on the surface and has higher uplift on both sides. When AP (> 10 um), the material removal mode gradually changes to brittle removal mode, resulting in cracks and cracks on the surface, which become more and more serious with the increase of cutting depth, so the grinding surface roughness gradually increases with the increase of cutting depth. However, when AP > 15 microns, the surface material of superfine cemented carbide grinding begins to powder and evenly smeared with Co phase, and the roughness value of grinding surface decreases gradually (see Fig. 1).

According to formula (3), the critical normal load of grinding crack nucleation of cemented carbide is related to the physical and mechanical properties of the material itself. The higher the fracture toughness or the lower the hardness of the material, the greater the critical normal load Pc of grinding surface cracking. Compared with the conventional structure cemented carbide with larger WC particle size, the ultra-fine cemented carbide has higher hardness and lower fracture toughness, and its Pc is much smaller in the grinding process. Under the same grinding conditions, the grinding surface of ultra-fine cemented carbide is easier to produce powdering.  Therefore, when the cutting depth reaches a certain value, the roughness of the grinding surface decreases gradually, and the Pc is much smaller in the grinding process. Under the same grinding conditions, the grinding surface of ultra-fine cemented carbide is easier to produce the powder. Therefore, when the cutting depth reaches a certain value, the roughness of the grinding surface decreases gradually.

Concluding remarks

(1) Under the same cutting depth, the grinding surface roughness of superfine cemented carbide increases with the increase of grinding wheel size. The surface roughness is low when grinding with a fine diamond grinding wheel.

(2) When grinding with the same size grinding wheel, the surface roughness of ultra-fine cemented carbide grinding increases with the increase of the cutting depth. When the cutting depth increases to a certain value, the grinding surface roughness decreases gradually.

(3) The influence of grinding parameters on the surface roughness of ultra-fine cemented carbide grinding can be attributed to the difference of material removal methods during grinding.

This is this week’s material weekly. I hope it will be helpful to you.

激情综合亚洲欧美调教-亚洲综合日韩精品国产-国产成人亚洲精品av大片-久草青青亚洲毛片在线视频| 欧美日韩精品视频免费下载-中文字幕一区二区三区伦理-一级特黄大片亚洲高清-午夜欧美日韩精品久久久久| 四虎精品高清在线观看-日韩有码国产中文字幕-国产一区二区三区亚洲污在线观看-亚洲av永久久无久之码精| 男人的精品天堂一区二区在线观看-婷婷久久香蕉毛片毛片-久久视频在线观看夫妻-亚洲国产一区久久yourpan| 国产精品自拍射精视频-蜜桃视频在线中文字幕-黑人泄欲一区二区三区-国内少妇无套内射精品视频| 亚洲成人av综合在线-日韩精品久久久中文字幕人妻-国产精品无套白嫩剧情-五月婷婷久久激情综合| 日韩国产自拍在线视频-亚洲av午夜激情在线播放-午夜福利你懂的在线观看-少妇特殊按摩高潮惨叫| 日韩视频精品在线播放-国产91亚洲精品久久-亚欧洲乱码视频在线观看-亚洲国产成人91精品| 欧美日韩国产在线三级-少妇人妻精品一区二区三-调教熟妇女同在线观看中文字幕-亚洲成av人片一区二区三区不卡| 国内自拍视频在线观看h-亚洲美女性生活一级片-香蕉久久夜色精品国产成人-亚洲国产成人久久综合人| 成人久久一区二区三区精品-日本伦理在线一区二区三区-全亚洲最大黄色在线网站-国产免费午夜福利片在线| 亚洲视频在线观看第一页-精品偷拍另类欧美日韩-日韩高清在线一区二区三区-久久天天操狠狠操夜夜av| 麻豆视频传媒在线免费看-亚洲性码不卡视频在线-岛国av色片免费在线观看-久久久国产精品视频大全| 91精品国产精品国产-国产成人一区二区免av-亚洲av激情在线观看-一区二区三区亚洲精品在线观看| 成人在线永久免费视频-日本理论电影一区二区三区-中文字幕成人av电影-91麻豆精品国产91久久麻豆| 亚洲欧美日韩另类影院-亚洲一区二区三区精品春色-精品人妻久久一品二品三品-人妻有码av中文字幕久久午夜| 国产精品一区二区三区四区-日本毛茸茸的丰满熟妇-中文字幕久久中文字幕久久-国产成人三级一区二区在线观看| 国产一区二区三区四区在线播放-国语精品国内自产视频-可以免费看黄的网久久-久久久亚洲av三吉彩花| 女优av天堂中文字幕-国产亚洲精品成人av久-国产黄三级三级三级三级一区二区-日本高清视频不卡一区二区| 四虎国产在线播放精品免费99-一区二区三区中文字幕日本-91国偷自产中文字幕久久-青青草一级视频在线观看| 日韩av不卡一区二区-国产白丝精品91久久-午夜福利理论片在线播放-国产粉饼哪个牌子好用| 欧洲熟女乱色一区二区三区-人妻中文字幕一区二区在线视频-亚洲码欧洲码一区二区三区四区-日本片在线美女视频骚货| 蜜臀av午夜精品福利-日韩精品av在线一区二区-丰满熟女人妻一区二区三区-懂色日韩欧美国产亚洲| 亚洲人妻精品中文字幕-国产黄色性生活一级片-日韩人妻系列在线视频-精品国产看高清av毛片| 男人天堂色男人色偷偷-国产内射在线干得爽到语无次-国产成人亚洲欧美二区综合-精品欧美高清视频观看| 日韩中文有码字幕在线观看-黑人国产一区二区三区-久久国产精品久久精品-国产激情在线一区二区三区| 人妻av久久人妻水蜜桃-国产一区视频在线二区-五月婷六月丁香久久综合-国产精品中文字幕有码| 色哟哟中文字幕在线播放-人人妻人人澡人人狠人人爽-国产午夜福利精品一区二区三区-性生活在线免费视频观看| 国内自拍视频在线观看h-亚洲美女性生活一级片-香蕉久久夜色精品国产成人-亚洲国产成人久久综合人| 国产视频深夜在线观看-在线播放亚洲欧洲亚洲-不卡日韩av在线播放-国产午夜视频在线观看| 日本一区二区三区视频高清-国产麻无矿码直接观看-国产精品久久久久久无-日韩精品不卡在线视频| 台湾香港a毛片免费观看-国产美女口爆吞精的后果-亚洲天堂成人免费在线-国模在线视频一区二区三区| 最近中文字幕国产精品-国产一级片黄片免费观看-日本一区二区三区日韩欧美-亚洲一区电影网站在线观看| 日韩黄片av在线免费观看-久久精品国产亚洲av色哟哟-亚洲第一中文字幕少妇-91久久精品国产性色tv| 青草视频在线观看精品综合-黑人巨大精品欧美久久-日本理论三级在线观看-九九热九九热这里只有精品| 国产精品精品久久99-久久羞羞色院精品全部免费-日韩中文粉嫩一区二区三区-外国黄色三级视频网站| 亚洲av成人精品爽爽-国产麻豆91在线播放-国产精品久久精品久久精品-蜜臀久久综合一本av| 国产在线精品一区二区中文-亚洲小说欧美另类激情-97碰久日韩视频在线观看-日本一道本高清不卡区| 日韩在线免费av网站-免费啪视频一区二区三区在线观看-久操热在线视频免费观看-91亚洲国产成人精品性色| 人妻体内射精一区二区三区小视频-国产精品久久久久人人爽-日韩三级黄色一区二区三区-亚洲伊人色综合网收藏| 成人高清视频在线播放-91麻豆免费观看视频-久久婷香五月综合色吧-自拍自产精品免费在线|