Cemented carbide is a composite material composed of high-hardness refractory metal carbides and cemented metals. Because of its high hardness, wear resistance, and stable chemical properties, it is used in modern tool materials and wear-resistant materials. High temperature and corrosion resistant materials occupy an important position. At present, tungsten carbide-based hard alloys are the most widely used among the carbides produced in the world, with the largest output and the most extensive use. Among them, the WC hard alloy used in mines has been regarded as the “tooth” of the mine development, oil drilling and geological exploration industries, and has received extensive attention.
Mine rock drilling tools are composed of a metal base body and different geometric shapes embedded therein and different grades of WC hard alloy drill teeth according to different working conditions. Take pick-axle picks as an example, the working environment of the picks is harsh, and in addition to the abrasive wear under compression, bending, and high stress, it also bears an indefinite impact force, so carbides often occur during coal mining. The head is broken and falls off, which leads to premature wear and failure of the pick-up matrix, which makes the life of the pick-shaped picks much lower than the design life. Therefore, an excellent hard alloy for mining should have high strength, high hardness required for abrasion resistance and high toughness required for resistance to impact fracture.

Features And Preparation Of Tungsten Carbide Mining Tool 1

Tungsten Carbide Mining Tool Features

1.1 Wear resistance of WC alloy

The shearer of the shearer is in direct contact with the coal seam during the working process. The abrasive wear characteristics of the shearer are closely related to the coal seam structure and hardness. The hardness of the coal is low, generally 100 to 420 HV, but the coal often contains different hardness. Impurities such as quartz and pyrite (900 to 1100 HV) have high hardness and have a great influence on the abrasive wear characteristics of picks.
In most of the operating examples, wear resistance is a basic function of material hardness. The higher the hardness, the higher the abrasive wear resistance. Pure WC is very hard and similar to diamond. In cemented carbide, WC particles form a strong skeleton, so WC cemented carbides exhibit very high hardness. In addition, WC belongs to the hexagonal crystal system and has anisotropy in hardness. The Vickers hardness of the bottom surface {0001} and the edge surface {1010} is 2 100 HV and 1 080 HV, respectively. In the coarse-grained cemented carbide, the proportion of WC grains on the {0001} plane is high, and thus the carbide containing the coarse-grained WC shows higher hardness. At the same time, at a high temperature of 1 000°C, coarse-grained WC hard alloys have higher hardness than ordinary hard alloys and show good red hardness.
In the coal cutting process, WC particles are exposed on the surface of the cemented carbide after cemented phases of the cemented carbide in the tool nose protected by the built-up edge have been squeezed away or are carried away by abrasive scraping. Bonded phase-supported WC particles are easily crushed, destroyed and released. Due to coarse WC grains, the cemented carbide has a strong holding force with respect to the WC, and the WC grains are difficult to pull out and exhibit excellent wear resistance.

1.2 Toughness of WC Alloy

When the cutter bit cuts the coal rock, the cutter head is subjected to high-stress stress, tensile stress and shear stress under the action of the impact load. When the stress exceeds the strength limit of the alloy, the alloy cutter head will be fragmented. Even if the generated stress does not reach the strength limit of the cemented carbide, the fatigue cracking of the cemented carbide will occur under the repeated action of the impact load, and the expansion of the fatigue crack may cause the tool head to fall off or chipping. At the same time, when cutting the coal seam, the shearer pick produces high temperature of 600-800°C on the cutting surface, and the cutting cutting coal seam is a periodic rotary motion. The temperature rise is alternating, and the temperature increases when the cutter head contacts the coal rock. , cool down when leaving the coal rock. Due to the constant change of the surface temperature, the dislocation density increases and concentrates, and the surface of the serpentine pattern appears.
The depth of cracks and the rate of propagation decrease with increasing carbide grain size, and the morphology, direction, and depth of cracks also vary with WC grain size. The cracks in fine-grained alloys are mostly straight and small and long; coarse-grained alloy cracks are irregular and short. The cracks mainly extend at the weak grain boundary. In the coarse-grained cemented carbide, if the micro-cracks bypass the coarse-grained WC grains, they are zigzag-shaped and must have energy that matches the fracture area; if they pass through When WC grains are expanded, they must have considerable fracture energy. As a result, the coarse-grained WC grains have enhanced deflection and bifurcation of cracks, which can prevent the further propagation of micro-cracks and increase the toughness of the cemented carbide. With the same content of cementitious phase, the coarse-grained alloy has a thicker bonding phase, which is beneficial to the plastic deformation of the bonding phase, inhibits the extension of cracks, and shows good toughness.
Studies on the strength and structure of WC-Co cemented carbide also show that there is a certain rule between the strength of cemented carbide and the grain size of WC. When the cobalt content is constant, the strength of conventional low-cobalt alloys always increases as the grain size of WC in the cemented carbide becomes coarser, and the strength of the alloy with higher cobalt content peaks with WC grain coarsening.

2 Research Progress on Preparation Process of Mining WC Alloy

At present, tungsten carbide powders are generally prepared by the process of reducing tungsten oxide to obtain coarse tungsten powder, tungsten powder obtained by high-temperature carbonization to obtain coarse WC powder, and WC powder and Co powder through mixing, wet grinding and sintering. Among them, the choice of coarse WC powder preparation, sintering process and equipment directly affects the performance of the mine WC alloy.

2.1 Preparation of WC Powder

(1) Preparation of coarse tungsten powder

Luo Binhui’s test results show that the oxygen content of tungsten oxide raw material directly affects the particle size of tungsten powder. To produce ultra-fine tungsten powder, tungsten oxide with lower oxygen content should be selected as raw material (usually purple tungsten), and coarser tungsten powder should be selected for oxygen production. A high content of tungsten oxide (yellow tungsten or blue tungsten) is used as a raw material. The results of Zhang Li et al. showed that compared with yellow tungsten, the use of blue tungsten to obtain coarse-grain tungsten powder has no advantage in particle size and distribution. However, the surface micropores are less tungsten powders made from yellow tungsten, and the overall performance of cemented carbides is better. It is known that the addition of an alkali metal to tungsten oxide contributes to the long coarseness of the tungsten powder, but the residual alkali metal in the tungsten powder suppresses the growth of WC crystal grains. Sun Baoqi et al. used lithium-activated tungsten oxide for hydrogen reduction to prepare coarse tungsten powder. Based on the experimental results, he explored the mechanism of activation and grain growth. He believed that by adding volatile lithium salt, the volatile deposition rate during the reduction of tungsten oxide was accelerated, resulting in Tungsten grows at lower temperatures. Huang Xin added Na salt in WO 3 for intermediate temperature reduction. The particle size of tungsten powder is proportional to the amount of Na added. With the increase of Na addition, the number of large crystal grains increased from 50 to 100 μm.

(2) Classification of tungsten powder

Gao Hui believes that the classification of tungsten powder can effectively change the properties of powder and solve the problem of uneven thickness of powder. Reduce the difference between the minimum, maximum, and average particle diameters to produce a coarser, more uniform WC powder; due to the characteristics of tungsten, it is not easily broken, and moderate crushing is performed prior to classification to separate the agglomerated particles in the powder. , more effective separation of powder, improve the uniformity.

(3) Coarse WC Powder Preparation

Preparation of coarse-grained WC powders by high-temperature carbonization of coarse-grained tungsten powders is a classical and classical method. The coarse-grain tungsten powders are mixed with carbon black and then mixed into a carbon tube furnace. The carbonization temperature of coarse tungsten powders is generally about 1 600°C, and the carbonization time is 1 ~ 2 h. Due to carbonization at a high temperature for a long time, this method minimizes the lattice defects of WC and minimizes the microscopic strain, thereby improving the plasticity of WC. In recent years, the tungsten powder carbonization process has been continuously developed. Some cemented carbide production plants have begun to adopt advanced intermediate frequency induction furnaces for vacuum carbonization and hydrogenation.
Due to the phenomenon of sintering and growth of WC powder particles, WC particles grow thicker and thicker at high temperatures. In addition, the finer the original tungsten powder, the more obvious the phenomenon of high temperature and WC grain growth. It is based on this principle that the use of medium-grained tungsten powder and even fine-grained tungsten powders for high-temperature carbonization to obtain coarse-grained tungsten carbide. The use of tungsten powder (Fisher sub-sieve sixer, Fsss 5.61 to 9.45 μm) was reported in the literature. The carbonization temperature was 1 800 to 1 900 °C, and WC powder with Fsss 7.5 to 11.80 μm was obtained. Fine tungsten powder was used. (Fsss < 2.5 μm), carbonization temperature 2 000°C, WC powder with Fsss of 7 to 8 μm was prepared. Due to the large density difference between tungsten and WC, the tungsten particles convert to WC particles during the conversion from tungsten to WC.
The resulting WC particles contain large strain energy, and some of the WC particles burst as a result, and the WC particles become smaller after blasting. Huang Xin et al. adopted a two-step carbonization method. Since the first time was incomplete carbonization, the particle core part remained pure tungsten, and the surface layer of the particles had been carbonized completely. Pure tungsten could be recrystallized to consume part of the strain energy, thereby reducing grain cracking. The probability. Compared with the conventional one-step WC powder, the coarse-grained WC powder produced by the two-step method has a single phase composition and almost no W 2 C, WC (1-x) and other miscellaneous phases. Zhang Li et al. studied the effect of Co doping on the grain size and micro morphology of coarse and coarse WC powders. The results show that Co doping is beneficial to the increase of grain size and free carbon of WC powder and is beneficial to single crystals. WC powder. When the doping content of Co is 0.035%, the crystal integrity of the WC grains is significantly improved, showing a distinct growth step and growth plane.

(4) Coarse-crystal aluminum thermal process

The distinctive feature is that tungsten carbide can be used to directly produce tungsten carbide, and the tungsten carbide powder produced is particularly thick and carbonized. A mixture of tungsten ore and iron oxide is reduced with aluminum, while carbide is used for calcium carbide. As long as the charge is ignited, the reaction proceeds spontaneously, resulting in an exothermic reaction with a self-heating temperature of up to 2500°C. After the reaction is over, the reaction kiln and material are allowed to cool down. The lower part of the kiln will produce a WC-based block layer, and the rest will be metal iron, manganese, excess metal aluminum, and a small amount of slag. The upper slag layer was separated, the lower ingot was crushed, excess calcium carbide was removed by washing with water, iron, manganese, and aluminum were removed by acid treatment, and finally, WC crystals were sorted by gravity dressing. The WC produced by this process is ground to a micron level for use with a variety of different cemented carbides.

2.2 Sintering of WC Carbide

(1) Vacuum sintering

In the vacuum sintering, the wettability of the bonding metal to the hard phase is significantly improved, and the product is not easily carburized and decarburized. Therefore, many of the world’s famous cemented carbide manufacturers use vacuum sintering, and vacuum sintering in China’s industrial production has gradually replaced hydrogen sintering. Mo Shengqiu studied the preparation of WC-Co cemented carbide with low cobalt content by vacuum sintering, and pointed out that the process system in the pre-firing stage is the key to vacuum sintering of WC-Co cemented carbide with low cobalt content. At this stage, the impurities and oxygen in the alloy are eliminated, the volumetric shrinkage is relatively intense, and the density increases rapidly. The pre-burning vacuum in the 0.11 ~ 0.21 MPa alloy has better final performance. For coarse-grained WC-Co cemented carbides with cobalt content between 4% and 6%, for high strength, the pre-sintering temperature should be between 1 320 and 1 370 °C.

(2) Low pressure hot isostatic pressing

Vacuum sintered cemented carbide has a small amount of pores and defects. These pores and defects not only affect the performance of the material, but also tend to be the source of the fracture during use. Hot isostatic pressing technology is an effective method to solve this problem. From the early 1990s, low-pressure hot isostatic pressing sintering furnaces were introduced in some large enterprises in China, such as Jianghan Bit Factory, Zhuzhou Cemented Carbide Factory, and Zigong Cemented Carbide Factory; Low-pressure sintering furnaces independently developed by Beijing Iron and Steel Research Institute have been put into operation. use. The application of low pressure hot isostatic pressing reduces the porosity of the cemented carbide and the structure is dense, and improves the impact toughness of the alloy and improves the life of the cemented carbide.
Jia Zuocheng and other experimental results show that the low pressure hot isostatic pressing process is beneficial to the elimination of voids in the alloy and WC grain growth, and increases the flexural strength of coarse-grained WC-15Co and WC-22Co alloys. Xie Hong et al. studied the effects of vacuum sintering and low-pressure sintering on the properties of WC-6Co cemented carbides. The results show that the vacuum sintering material Vickers hardness 1 690kg / mm 2, the transverse rupture strength is 1 830 MPa, while the low-pressure sintered material Vickers hardness is increased to 1 720 kg / mm 2, the transverse rupture strength is 2140 MPa. Wang Yimin also produced WC-8Co alloys by vacuum sintering and low pressure sintering. The results show that the vacuum sintered material has a hardness of 89.5 HRA and a transverse rupture strength of 2270 MPa; and the low-pressure sintered material has an increased hardness of 89.9 HRA and transverse fracture. The strength is 2 520 MPa. The temperature uniformity of the sintering furnace is an important factor affecting the quality of high-performance carbide products. A large number of studies have simulated and optimized the temperature field in the sintering furnace. The literature proposes a piecewise simulation method that is consistent with the experimental results. The temperature distribution in the graphite tube is not uniform, which is mainly due to the unreasonable arrangement of the graphite boat and the sintered product and the structure of the graphite tube. In the test, optimization measures were proposed to reduce the surface temperature deviation of sintered products by approximately 10 K during the vacuum phase and within ±7 K during the gas heating phase, thereby improving the sintering quality.

(3) Spark Plasma Sintering (SPS)

A method of sintering under pressurized conditions using instantaneous and intermittent discharge energy. The mechanism of SPS sintering is still controversial. Scholars at home and abroad have conducted extensive research on this topic. It is generally believed that a discharge plasma is instantaneously generated when a direct current pulse is applied to an electrode, so that heat generated uniformly by each particle in the sintered body activates the surface of the particle, and sintering is performed by the self-heating effect of the inside of the powder. Liu Xuemei et al used XRD, EBSD and other test methods to compare the phase composition, microstructure and properties of the hard alloy materials obtained by hot press and spark plasma sintering. The results show that the SPS sintered materials have high fracture toughness. Xia Yanghua, etc. using SPS technology with an initial pressure of 30 MPa, sintering temperature 1 350 °C, holding 8 min, the temperature of 200 °C / min prepared carbide hardness of 91 HRA, transverse fracture strength of 1 269 MPa. The literature uses SPS technology to sinter WC-Co cemented carbides. It can produce WC- with relative density of 99%, HRA ≥ 93 and good phase formation and uniform microstructure under sintering temperature of 1270°C and sintering pressure of 90 MPa. Co Carbide. Zhao et al. of the University of California, USA prepared the binder-free cemented carbide by SPS method. The sintering pressure was 126 MPa, the sintering temperature was 1 750°C, and no holding time was obtained. A fully dense alloy was obtained but a small amount of W 2 C phase was contained. In order to remove impurities, an excess of carbon was added. The sintering temperature was 1 550°C and the holding temperature was 5 μm. The material density remained unchanged and the Vickers hardness was 2 500 kg / mm 2.
Spark plasma sintering as a new type of rapid sintering technology has broad application prospects. However, the research at home and abroad is still limited to the laboratory research stage. The sintering mechanism and sintering equipment are the main obstacles to its development. SPS sintering mechanism is still controversial, especially the intermediate processes and phenomena of sintering have yet to be further studied. In addition, the SPS equipment uses graphite as a mold. Because of its high brittleness and low strength, it is not conducive to high-temperature and high-pressure sintering. Therefore, the mold utilization rate is low. For actual production, it is necessary to develop new mold materials with higher strength and reusability than the currently used mold materials (graphite) in order to increase the bearing capacity of the mold and reduce the cost of the mold. In the process, it is necessary to establish the temperature difference between the mold temperature and the actual temperature of the workpiece in order to better control the product quality.

(4) Microwave sintering

A method in which microwave energy is converted into heat energy for sintering by using the dielectric loss of a dielectric in a high-frequency electric field, and the entire material is uniformly heated to a certain temperature to achieve densification and sintering. The heat is generated from the coupling of the material itself with the microwave, rather than from the external heat source. The Monika team studied the microwave sintering and traditional sintering densification of WC-6Co cemented carbides. The experimental results show that the degree of densification of microwave sintering is faster than that of traditional sintering. Researchers at the University of Pennsylvania studied the production of tungsten carbide products in the microwave sintering industry. They have higher mechanical properties than conventional products, and have good microstructure uniformity and low porosity. The microwave sintering process of WC-10Co cemented carbide by microwave sintering was studied in the omni-peak system. The interaction of microwave electric field, magnetic field and microwave electromagnetic field on WC-10Co cemented carbide was analyzed.
The lack of material properties data and equipment are two major obstacles to the development of microwave sintering technology. Without the data on the material properties of materials, one cannot know the mechanism of action with microwaves. Due to the strong selectivity of microwave sintering furnaces for products, the parameters of microwave ovens required for different products are very different. It is difficult to manufacture microwave sintering equipment with a high degree of automation, with variable frequency and automatic tuning functions, which is a bottleneck restricting its development.

Leave a Reply

Your email address will not be published. Required fields are marked *

日本一区二区三区四区黄色-91在线国产经典观看精品-亚洲一区二区三区免费不卡-av免费在线观看蜜臀| 国产老熟女乱子一区二区-欧美日本中国一区二区-欧美日韩国产午夜精品-青青草视频在线观看入口| 九九热这里只有精品在线免费视频-色一情一乱一乱一十九区-国产午夜福利视频在线观看-久草免费手机在线视频观看| 久热这里只有精品视频66-国产资源精品中文字幕-亚洲免费视频一区二区三区四区-亚洲国产特一特二区精品分布| 亚洲午夜福利在线看片-草草影院在线观看国产-中文字幕在线国产有码-精品99成人午夜在线| 亚洲天堂av中文在线-亚洲精品有码中文字幕网络-在线播放国产一区二区不卡-香港毛片免费观看视频| 日本人妻中文字幕有码视频-男女啪啪视频免费观看一区-青青草原综合在线视频-极品人妻少妇精品一区二区| 国产成人精品一区二区日出白浆-亚洲女优大片在线观看-明星换脸av一区二区三区-四虎影院国产精品久久| 国产精品一区二区三区av麻-蜜桃传媒免费在线播放-久久亚洲中文字幕精品-国产精品白嫩极品在线看| 高清国产av一二三四-少妇激情高潮视频网站-被公么玩弄邻居人妻中文字幕-亚洲免费成人av在线| 精品淑女少妇av久久免费-欧美激情亚洲精品一区-九九热在线视频观看精品-亚洲天堂激情av在线| 少妇人妻偷人偷人精品-国产精品黄色在线播放-亚洲熟伦熟女新五十路熟妇亚洲-国产综合91精品百人斩| 极品尤物在线免费观看-超碰九七精品在线观看-午夜爱爱免费观看视频-日本免费人成黄页在线| 久久99精品成人免费毛片-中文字幕日韩精品欧美-免费观看黄片一区视频-国产亚洲蜜臀av在线观看| 在线观看亚洲天堂成人-亚洲大片久久精品久久精品-日韩在线免费观看毛片-成年大片免费视频播放| 久久99精品成人免费毛片-中文字幕日韩精品欧美-免费观看黄片一区视频-国产亚洲蜜臀av在线观看| 国产福利一区在线观看蜜臀av-最新天堂中文在线官网-成人精品天堂一区二区三区-国产精品久久久久久久人貌| 久久精品中文字幕一区二区-日本夫妻性生活视频播放-综合久久精品亚洲天堂-日韩中文字幕不卡久久| 少妇被搞高潮在线免费观看-亚洲av成人精品小宵虎南-日韩性生活免费看视频-日韩黄色大片在线播放| 亚洲丁香婷婷久久一区二区-少妇高潮乱语对白自拍-99偷拍在线视频精品-天堂精品中文字幕在线| 少妇被爽到高潮喷水在线播放-国产精品中文字幕在线不卡-中文字幕不卡一区二区三区-精品国产一二三区在线观看| 欧美日韩国产在线三级-少妇人妻精品一区二区三-调教熟妇女同在线观看中文字幕-亚洲成av人片一区二区三区不卡| 中文字幕亚洲综合精品一区-久久好视频久久这里有精品-国产在线传媒高清视频-日韩精品一区二区亚洲av失禁| 日韩av高清不卡一区二区-国产亚洲性色av大片久久香蕉-国产亚洲欧美韩国日本-国产精品国产三级国产普通话对白| 欧美黄色在线观看免费-日本高清精品一卡二卡-日本综合精品一区二区在线-国产精品伦人一久二久三久| 青草精品在线视频观看-色呦呦在线观看中文字幕-国产一区二区日本在线观看-草青青在线视频免费观看| 五月婷婷丁香综合入口-日本少妇免费中文字幕-96青草视频在线观看-中文字幕成人精品久久不卡| 久久都是精品久久都是精品-精国精品一区二区成人-亚洲品质自拍在线观看-中文 字幕乱码高清视频| 一区二区三区四区蜜桃av-国产av无套内射成人久久-亚洲第一大片一区二区三区三州-国产福利黄色片午夜在线观看| 精品久久激情中文字幕-扒下语文老师的丝袜美腿-日韩欧美精品在线免费看-国产成人亚洲精品在线| 日韩成av在线免费观看-中文字幕亚洲第一精品-亚洲欧美日韩国产在线-国产精品国精品国产免费| 国产精品视频午夜福利-一本大道久久综合一区-成年深夜福利在线观看-国产传媒免费在线视频| 精品人伦一区二区三区蜜桃-中文字幕久久人妻熟人妻-中文字幕av乱码在线看-久久精品国产亚洲妇女av| 98人妻精品一区二区久久-五月婷婷六月丁香久久综合-国产精品手机在线免费观看-亚洲国产日韩欧美综合| 91久久国产综合蜜桃-深夜激情在线免费观看-免费观看国产在线视频不卡-天堂在线精品免费亚洲| 中文字幕日韩有码av-麻豆国产成人av高清在线-可以免费观看的av毛片-久久这里只有精品国产亚洲| 成人精品一区二区三区不卡-十八禁啪啪啪一区二区三区-后入黑丝美女在线观看-国产熟女啪啪免费视频| 2023年久久国产精品-亚洲中文字幕二区在线观看-人人妻人人玩人人澡人九色-午夜精品福利视频网站| 久热99在线视频免费观看-黄片视频在线免费观看国产-国产精品av国产精华液-av在线男人的免费天堂| 久久精品国产普通话对白-丰满人妻中文字幕一区二区-国产日本精品视频在线观看-香港免费毛片在线观看| 在线播放中文字幕国产精品-亚洲av成人免费在线观看-国产男女激情视频免费观看-亚洲av黄片一区二区三区|