When WC grains in cemented carbide are less than 0.5 μ m, the finer the grains are, the fewer the defects are, and the higher the bending strength and hardness are The particle size of WC powder used to produce ultrafine cemented carbide is much smaller than that of WC powder used in general cemented carbide. The WC powder has high activity and is easy to cause grain growth in the sintering process, which is one of the crack sources.

At present, there are two main methods to control the grain size:

First, a new sintering process is adopted. The results show that the densification of dozens of nano WC Co composite powders can be completed after sintering at 1400 ℃ for 30s, and the grain size is 0.2 μ m, but if the sintering time is extended to 60s, the grain size will grow rapidly to 2.0 μ M. The new sintering processes that can be used for nano WC Co cemented carbide composite powder mainly include microwave sintering, hot isostatic pressing sintering, discharge plasma sintering and two-stage sintering.

Second, adding inhibitors of grain growth to inhibit grain growth, VC, TAC and Cr3C2 are often used inhibitors.

In this paper, the inhibition mechanism, the factors affecting the effect of inhibitors, the way of adding inhibitors, the commonly used inhibitors, the development of the latest inhibitors and the influence of inhibitors on the comprehensive properties of alloys are introduced.

Application of Grain Growth Inhibitors in Cemented Carbide 2

Inhibition mechanism and influencing factors of inhibitors

The driving force for the grain growth of cemented carbide comes from the reduction of surface energy. The grain growth of WC is mainly through the dissolution precipitation mechanism of WC, that is, small grain WC dissolves in the liquid phase and precipitates on the surface of large grain WC. For WC Co cemented carbides, the coarsening of WC grains can be limited by the addition of grain growth inhibitors.  

The addition of inhibitors slows down the dissolution precipitation rate of WC, and there are three inhibition mechanisms:

1. The inhibitor adsorbs on the surface of carbide particles, which reduces the surface energy of WC and the solubility of WC in liquid phase.

2. The inhibitor dissolves in liquid CO, which slows down the growth of WC through liquid recrystallization.

3. The migration of WC interface was hindered by the segregation of inhibitors along WC / WC interface, which prevented the aggregation and growth of WC particles.

The inhibition effect of inhibitors is determined by the following factors:

1. Decreasing the particle size of WC powder increases the grain boundary area of WC Co. inhibitors can be widely distributed on the surface of WC, but they can not be increased indefinitely. Their limit value depends on their saturation concentration in the bonding phase.

2. Cobalt content. With low content of binder and short free stroke, the inhibitor is easy to play its role at a certain temperature.

3. Uniformity of powder mixing. The uneven distribution of the binder phase in the mixed powder will lead to the difference of the effect area of inhibitors on WC grain growth in the sintering process; the uneven distribution or large size of the inhibitors in the mixed powder will lengthen the diffusion route required by the inhibitors

4. Alloy sintering temperature. With the increase of sintering temperature, the amount of liquid phase and the content of grain growth inhibitor need to be increased in order to keep the high concentration of inhibitor in the liquid phase Therefore, the smaller the powder size, the lower the cobalt content, the more uniform the powder mixing and the lower the sintering temperature are, the better the inhibition effect of the inhibitor is.

Application of Grain Growth Inhibitors in Cemented Carbide 3

Adding ways of grain growth inhibitor

Inhibitors are mainly added in three ways:

1. WC, CO and grain growth inhibitor were mixed in the wet grinding process.

2. Before w carbonization, oxide corresponding to grain growth inhibitor was mixed.

3. The third method is to wet mix the salt solution of the inhibitor with blue tungsten or yellow tungsten, and form coating powder with blue tungsten or yellow tungsten before reduction, and then conduct further thermal decomposition and reduction.

Application of Grain Growth Inhibitors in Cemented Carbide 4

Types of grain growth inhibitors

Transition metal carbides

Transition metal carbides are common inhibitors of grain growth. The effectiveness of transition metal carbides in inhibiting WC grains is related to their own thermodynamic stability. The order of their thermodynamic stability is VC > Cr3C2 > NBC > TAC > tic > ZrC > HFC. However, each kind of carbide has a maximum amount that can be added, which has no further effect on inhibiting the growth of WC grains. At a certain temperature, the amount of carbide additives depends on the saturation concentration of the carbide in the binder phase and the content of the binder phase Table 2 shows the solubility of various additives in CO phase. It can be seen from the table that VC and Cr3C2 have the highest solubility in CO phase and they have the lowest binary eutectic temperature, so they are widely used as WC Co grain growth inhibitors.

Application of Grain Growth Inhibitors in Cemented Carbide 5

Rare earth element

Rare earth element is one of the common additives, which can inhibit the grain growth, improve the structure distribution, purify the grain boundary, and play an effective role in strengthening and toughening the cemented carbide. At the same time, rare earth can also reduce the sintering temperature of cemented carbide, which can solve the contradiction between controlling grain growth and Sintering Densification. the increase of the macro compressive stress on the alloy surface is also an important reason for the increase of the strength of WC Co cemented carbide by the addition of rare earth oxides.

Boron and phosphorus

It is found that the sintering temperature of the cemented carbide with boron can be reduced to 1340 ℃, with the decrease of sintering temperature, the micro grains of the alloy are obviously refined, which is conducive to the improvement of the alloy performance, and the addition of boron has little effect on the wettability of the bonding phase and WC phase, and the bending strength of the alloy is not affected. The sintering temperature of WC Co can be reduced to 1050-1100 ℃ by adding a small amount of Ni and P powder. The mechanism is that the eutectic temperature of Ni-P is far lower than the melting point of Co. after adding Ni and P, the liquid phase can appear at a lower temperature, which makes the dissolution and precipitation of solid particles and the formation of framework occur in advance, and the sintering process is more sufficient, thus inhibiting the growth of WC grains.

Copper molybdenum metal inhibitor

The addition of a small amount of Cu to wc-13fe / Co / Ni cemented carbide can refine the spheroidized WC grains. This is mainly because Cu will dissolve into the Fe / Co / Ni binder during the sintering process, reducing the solubility of WC in the binder, thus reducing the rate of grain growth during the dissolution re precipitation process. And copper also spheroidizes WC grains. In the sintering process of cemented carbide, molybdenum is coated around the cemented phase, which improves the wettability between the cemented phase and the cemented phase, so as to refine the particles of cemented phase

Effect of grain growth inhibitor on properties of alloy

The effect of grain growth inhibitors on the properties of the alloy is mainly reflected in the hardness and bending strength of the alloy Different additives have different mechanisms of inhibiting grain size, so different inhibitors of grain growth have different effects on properties.

Transition metal carbides

The addition of VC, Cr 3C 2 and other additives can effectively improve the heat resistance and wear resistance of WC Co cemented carbide. Moreover, the high temperature strength and high temperature hardness of the alloy can be effectively improved when the additive is appropriate, but the room temperature strength of the alloy can be reduced and the alloy becomes brittle. Therefore, the amount of additives must be controlled within a certain range For example, for WC-6% CO and WC-10% Co alloys, the addition of cr2c3 reduced the room temperature bending strength of the alloy. When the content of Cr 2C 3 is 0.3% ~ 0.5% (mass fraction of CO content), the room temperature bending strength of the high Co alloy will not be affected obviously, but for the low Co alloy, the room temperature bending strength will be decreased obviously. Adding TAC and NBC will result in the same result The effect of VC on the microstructure and properties of wc-6.5% Co cemented carbides was found. It was found that VC inhibited the growth of WC grains, which resulted in obvious grain refinement and narrowed the distribution of grain size. The grain size decreased from 0.5-1 μ m without adding VC to 0.15 μ m with adding 2.0% VC. At the same time, the hardness of the alloy is greatly improved by adding VC, and the maximum value is 94.1 HRA when VC content is 2.0%. But it also reduces the strength of the alloy When VC content is 0.5%, the hardness and toughness of the alloy are 93.0hra and 11.2MPa · M 1 / 2, and the comprehensive properties are the highest. The addition of TAC can not only prevent the WC grains from growing too much, but also reduce the carbon content of the alloy

Rare earth element

The hardness of WC-20 (Fe / Co / Ni) alloy increased with the increase of rare earth content. The addition of rare earth can improve the properties of w-co-ti alloy, especially improve the impact resistance of Shejin. At the same time, rare earth can inhibit the grain aggregation and growth of (Ti, w) C solid solution and refine the grain.  When rare earth oxide is added to WC Ni alloy, the strength of bonding phase Ni increases due to dispersion strengthening of rare earth oxide. When the rare earth content is 1.2% ~ 1.6% of bonding metal content, the bending strength of the alloy reaches the maximum value (1680mpa when CeO 2 is added, 1900mpa when Y2O3 is added). The bending strength of WC-8% Co alloy is increased to a certain extent by adding 0.25% ~ 1.00% of the mixed rare earth oxide, and it can be increased by 11.5% when adding 0.25% ~ 0.50% of the rare earth oxide, but the excessive addition of rare earth will lead to the decrease of the bending strength. Therefore, the bending strength of cemented carbide with rare earth elements can be greatly improved.

Cu&Mo metal inhibitors

Adding a small amount of copper into the cemented carbide can not only improve the strength of the alloy, but also improve the impact toughness of the alloy.

When a small amount of copper is added to WC-13% Fe / Co / Ni, the hardness of the alloy decreases, while the bending strength increases greatly. When the amount of copper is about 0.8%, the bending strength and hardness of the alloy are 2370 MPa and hra84.4 respectively. See Table 3 below. When Mo was added to WC Co, the bending strength and India increased with the increase of Mo addition. The bending strength reached the maximum value when Mo addition was 5%, and reached the peak value of 19.25gpa when Mo addition was 7.5%. However, when the amount of Mo is more than 5%, the bending strength decreases gradually, which is due to the embrittlement of the sample caused by the presence of intermetallic compound CO3(Mo, w)3C.

Aplicación de inhibidores del crecimiento de granos en carburo cementado 6

国产精品高潮呻吟久久av嫩-青青草免费公开在线观看视频-亚洲欧美日韩另类综合视频-国产三级在线观看精品| 亚洲日本精品国产第一区二区-国产一级二级三级大胆视频-片黄片色日韩在线观看免费-五月综合婷婷中文字幕| 日韩精品成人一区二区三区-亚洲综合中文字幕第一页-久久伊人亚洲中文字幕-花季传媒视频无限制观看| 日韩成人av在线影院-亚洲五月天久操视频在线观看-最新国产AV无码专区亚洲-欧美日韩大香蕉在线视频| 欧美激情一级欧美精品-国产一区二区在线免费视频观看-日韩不卡视频免费在线观看-国产成人深夜在线观看| 国产成人精品一区二区日出白浆-亚洲女优大片在线观看-明星换脸av一区二区三区-四虎影院国产精品久久| 亚洲丁香婷婷久久一区二区-少妇高潮乱语对白自拍-99偷拍在线视频精品-天堂精品中文字幕在线| 四虎精品高清在线观看-日韩有码国产中文字幕-国产一区二区三区亚洲污在线观看-亚洲av永久久无久之码精| 欧美日韩国产激情综合-九九精品国产亚洲av日韩-国产午夜激情免费视频-日本厕所偷拍尿尿视频| 97中文字幕一区二区三区-国产精品亚洲av无人-亚洲国产精品自产拍久久-成人深夜福利在线视频| 白白色视频国产在线观看-美女高潮无套内谢视频日韩-成人能看的性生活视频大全-中文字字幕在线亚洲乱码| 亚洲av成人午夜福利在线观看-日韩精品成人影院久久久-国产在线高清不卡一区-激情五月另类综合视频| 国产精品精品久久99-久久羞羞色院精品全部免费-日韩中文粉嫩一区二区三区-外国黄色三级视频网站| av天堂免费中文在线-91麻豆国产综合精品久久-日韩av在线播放高清-台湾佬自偷自拍情侣在线| 精品少妇人妻av蜜桃-成年人网站在线免费播放不卡-免费黄色片成人国产精品-蜜桃中文字幕在线视频| 精品人妻一区二区三区久久91-久久精品亚洲国产av搬运工-日本熟女人妻一区二区三区-亚洲国产精品高清线久久| 午夜男女靠比视频免费-欧美激情影院狂野欧美-国语淫秽一区二区三区四区-国产成人av区一区二区三泡芙| 日韩人妻毛片中文字幕-国产精品亚洲综合第一页-国产精品久久亚洲av-亚洲国产精品一区二区不卡| 2020天天操夜夜操-亚洲色图视频在线观看,-亚洲色图专区另类在线激情视频-岛国精品毛片在线观看| 成人精品一区二区三区不卡-十八禁啪啪啪一区二区三区-后入黑丝美女在线观看-国产熟女啪啪免费视频| 亚洲日本国产一区二区三区-日日噜噜夜夜狠狠免费-亚洲不卡在线视频观看-亚洲成年网站青青草原| 久久成人av一区二区三区-人妻一区二区三区久久丰满-日韩在线播放视频不卡-亚洲成熟女人一区二区三区| 人妻中文字幕一区二区三区-国产精品丝袜久久亚洲不卡-久久伊人精品色婷婷国产-日韩中精品文字幕在线一区| 精品视频人妻少妇一区二区三区-人妻中文字幕一二三区-日本老熟妇成熟老妇人-东京热国产精品二区三区| 少妇人妻上班偷人露脸-欧美中文字幕乱码视频-欧美韩日本一本交道免费-国产一区,二区,三区免费视频| 成a级人在线观看网站免费看-久久久精品国产亚洲av水蜜桃-亚洲第一狼人在线观看-黄色欧美精品一区二区三区| 日本一区二区三区四区黄色-91在线国产经典观看精品-亚洲一区二区三区免费不卡-av免费在线观看蜜臀| 少妇裸淫交视频免费看-欧美日韩中文字幕第一页-91精品看黄网站在线观看-国产精品一区二区三区色噜噜| 久久精品中文字幕久久-国产尤物精品在线观看-久久精品久久精品亚洲国产av-熟妇人妻中文字幕在线| 日韩成人大片一区二区三区-国产一级淫片av免费-18禁免费观看网站入口-国产黄色特级片一区二区三区| 亚洲国产一区二区精品专-人妻被黑人侵犯中文字幕夜色-国模午夜写真福利在线-成人自拍偷拍在线观看| 国产在线观看不卡一区二区-国产女人在线观看视频射精91-91尤物在线视频观看-欧美无遮挡国产欧美另类| 国产熟女老阿姨毛片看爽爽-精品少妇人妻久久免费-韩国午夜福利片在线观看-西川结衣在线中文字幕| 精品人妻一区二区三区免费-亚洲国产精品久久一区二区-国内久久偷拍视频免费-蜜桃视频在线观看网址| 激情综合网激情国产av-2021日韩午夜影院-精品一区二区三区少妇蜜臀-人妻交换av一区二区| 人日本中文字幕免费精品-日本口爆吞精在线视频-玖玖玖玖视频在线观看-国产精品内射在线播放| 久久综合九色综合久久-在线看日韩欧美中文字幕-国产成人亚洲精品青草天美-91亚洲中文天堂在线观看| 少妇一级aa一区二区三区片-欧美欧美欧美欧美一级片-91在线观看视频下载-自拍视频在线观看一区二区| 精品人伦一区二区三区蜜桃-中文字幕久久人妻熟人妻-中文字幕av乱码在线看-久久精品国产亚洲妇女av| 日韩亚洲分类视频在线-熟妇人妻久久中文字幕电-久久麻传媒亚洲av国产-精品丰满熟妇高潮一区| av网站在线观看网站-最新国产欧美精品91-国产一区二区三区在线导航-日韩高清在线中文字幕一区|