Mining pick is one of the vulnerable parts in coal mining and roadway driving machinery, and it is the main tool for coal falling and coal breaking. Its performance directly affects the production capacity of coal mining machinery, power consumption, working stability and the service life of other related parts. With the increase of people’s demand for energy, especially for coal, in order to improve the mining efficiency, the power of the shearer is increasing, and the quality of the pick is required to be higher and higher. As the material of the shearer pick, it is required to have higher strength, hardness and wear resistance, bending strength and corrosion resistance.

Working process of shearer pick

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 2

Under the action of the front edge of the pick, the coal is broken and the large block is peeled off at the same time. At the moment when the tip contacts the coal, there are elastic and plastic deformation in the contact range of the tip. With the increase of the contact stress, when the strength limit is exceeded, the core is crushed into very fine powder to form a dense core, which is composed of the crushed coal under pressure. With the advance of the cutting tool, the dense core gradually grows and accumulates energy, and the cutting resistance also increases. The dense core compresses the front coal area and makes this part produce elastic deformation. Because the ore body around the dense core forms the stress state area, it actually plays a role in changing the geometry of the pick cutter head. When the contact stress of the cutter tip increases to the limit value, the dust in the area before the dense core ejects at a high speed, driving the small pieces to peel off.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 3

Failure form

The main failure forms are the invalidation of alloy cutter head, chipping of cutter head, wear of alloy cutter head and gear body. In some working conditions, the failure of pick is often caused by the fracture of gear body. As the mechanical performance of the pick body directly affects the service life of the pick, it is of positive significance to select the material and effective heat treatment method of the pick body reasonably to reduce the wear and fracture of the pick, reduce the consumption of the pick of the shearer, improve the operation rate of the shearer and increase the comprehensive economic benefits of the production of the shearer.

Wear and fracture failure

In the process of cutting coal seam, the pick has strong friction and abrasive wear with the coal seam. The most stressed point of the pick is at the head of the working part of the pick, where the wear is the most serious, resulting in the wear and failure of the pick pants. In the actual coal production, about 50% of the pick failure is caused by wear.

Breaking and invalidation of cemented carbide tooth head

The invalidation of cemented carbide is related to the hardness of ore in coal and rock: when the pick cuts coal and rock, if the hard ore in coal and rock is encountered, the cutter head is in the state of high-pressure stress, and it will bear high shear stress at the place where the contact between the cutting edge and coal and rock is poor, and it is in the state of tensile stress. When the tensile stress exceeds the strength limit of the alloy, the cutter head will break.

related to the poor brazing quality of tooth head.

For example, there are sand inclusions and microcracks in the weld, which cause the shear strength of the weld to be low. The abscission of cemented carbide is also related to the unreasonable size of weld gap. The use of less solder during brazing results in the loosening of cemented carbide head and the abscission of tooth head.

related to the low hardness and poor wear resistance of the working part

From the point of view of the material of the pick pant body, the reason for the invalidation of the carbide cutter head is related to the low hardness and poor wear resistance of the working part of the pick magazine body. The excessive wear of the part of the pick supporting the carbide results in the insufficient supporting force and the invalidation of the carbide. Therefore, by improving the hardness of the working part of the pick and the quality of brazing, the invalidation of cemented carbide can be avoided.

Do You Know the Cause of Failure of Mining Pick and the Way to Improve Its Performance? 4

Performance improvement method

1. According to the hardness index of coal and rock, the corresponding grade of alloy cutter head is selected. Generally, the compressive strength of coal or coal rock roadway can be selected with less Co. the compressive strength of roadway surrounding rock should adopt the use of advanced technology such as limited or manufacturing composite alloy material spraying to improve the impact resistance.

2. The manufacturing process shall be in strict accordance with the design requirements, to ensure the matching between the pick and the gear holder, to ensure that the tool can rotate freely in the gear holder, to avoid the phenomenon of eccentric wear, the automatic grinding function, to maintain the normal wear of sharp blade and even cutting teeth, in the cut state. Brazing and heat treatment process. Brazing and heat treatment process is one of the key technologies for cutting quality of pick.

3. A layer of niobium carbide hard alloy is deposited on the surface of the coal pick steel machine by using the hardfacing technology to obtain the hardfacing wear-resistant layer with metallurgical structure with the base. Niobium carbide is distributed on the iron-based martensite and retained austenite intensively in the trading net of Chinese shearer, which protects the collective from wear. The Hardmetals with high hardness in the hardfacing layer and a large number of metallographic structures that play the role of wear-resistant framework make the hardfacing layer have high wear-resistance.

4. Thermal spraying can heat a linear or powdery material to a melting or semi melting state and accelerate the formation of high-speed droplet by means of heat sources such as flame, arc or plasma, spray to the substrate to form a coating on it, which can strengthen the surface of the material and improve its wear-resistant and corrosion-resistant properties.

5. Plasma cladding is a new material surface modification technology which uses plasma beam as heat source to obtain excellent wear resistance, corrosion resistance, heat resistance, impact resistance and other properties of metal surface. Plasma cladding is a rapid non-equilibrium solidification process, which has many strengthening effects such as supersaturated solution strengthening, dispersion strengthening and precipitation strengthening.

6. The brazing and heat treatment process of the pick is one of the key technologies to ensure the quality of the pick. At present, the brazing and heat treatment of pick are integrated technology. It is heated by vacuum furnace, so that the brazed pick can be directly quenched without air cooling, and the brazing and heat treatment can be completed once. It can avoid the oxidation phenomenon of the traditional brazing surface contacting with the air, ensure the direct contact between the melted solder and the brazing surface, and ensure the welding quality; at the same time, because the brazing and heat treatment are completed once, it can avoid the embrittlement of the alloy head and the reduction of the weld strength caused by the two heating.

粉嫩小粉嫩小国产小视-老熟妇人妻久久中文字幕麻豆网-蜜臀av在线播放国产-成年人的三级视频网站| 精品久久激情中文字幕-扒下语文老师的丝袜美腿-日韩欧美精品在线免费看-国产成人亚洲精品在线| 日本一区二区三区乱在线视频-国产精品一区二区精品视频-日本人妻系列在线免费看-国产成人高清三级视频| 最新国产精品欧美日韩-日韩孕妇孕交在线视频-亚洲欧美日韩国产成人在线-欧美老熟妇性视频在线观看| 精品久久激情中文字幕-扒下语文老师的丝袜美腿-日韩欧美精品在线免费看-国产成人亚洲精品在线| 亚洲一级特黄大片做受-国产91喷潮在线观看-日本不卡一区二区三区四区-在线观看高清视频一区二区三区| 激情六月综合激情六月-韩国国产日韩在线观看视频-久久精品国产亚洲av高清色-亚洲熟女乱码一区二区三区| 97视频在线观看精品在线-久久精品欧美日韩一区麻豆-亚洲精品在线少妇内射-国产在线一区二区三区三州| 九九热在线精品视频免费-日韩高清免费在线视频-熟女快要高潮了在线观看-亚洲午夜福利视频一级| 97中文字幕一区二区三区-国产精品亚洲av无人-亚洲国产精品自产拍久久-成人深夜福利在线视频| 射女人进去视频在线观看-91麻豆国产在线视频-久久国产精品99精品国产不卡-中文字幕欧美日韩国产| 国产韩国精品一区二区三区-久久精品人妻一区二区三区av-黄片视频在线观看欧美-国产成人自拍在线视频| 亚洲日本国产一区二区三区-日日噜噜夜夜狠狠免费-亚洲不卡在线视频观看-亚洲成年网站青青草原| 亚洲香蕉久久一区二区三区四区-国产夫妻内射一级一片-成人午夜福利片免费观看-一区二区三区四区黄色网| 最新国产精品欧美日韩-日韩孕妇孕交在线视频-亚洲欧美日韩国产成人在线-欧美老熟妇性视频在线观看| 久热99在线视频免费观看-黄片视频在线免费观看国产-国产精品av国产精华液-av在线男人的免费天堂| 少妇人妻午夜精品视频-亚洲乱妇老熟女爽到潮的片-最新国产黄色一区二区-亚洲一区国产精品喷潮| 国产亚洲欧美日韩俺去啦-91香蕉国产极品在线播放-国产夫妻生活自拍视频-永久免费的成年视频网| 99久久国产自偷自自偷蜜月-日韩熟女激情中文字幕-亚洲狼人社区av在线观看-四虎成人精品国产永久| 久久一日本道色综合久久大香-欧美午夜福利视频网站-亚洲av午夜精品一区二区-日韩精品区一区二区三区激情| 国产视色精品亚洲一区二区-激情艺术中心国产精品-国产农村一级特黄真人片-免费观看午夜视频在线| 国产精品亚洲精品日韩精品-狠狠爱婷婷网五月天久久-国产精品激情成色在人-国产农村妇女精品三级一区二区| 国产成人自拍视频精品-丝袜美腿亚洲一区二区刘亦菲-91精选国产在线视频-欧洲美熟女乱又伦免费| 国产成人高清视频在线观看免费-人妻精品一区二区在线视频-国产成人一区二区三区精品久久-农村肥白老熟妇20p| 精品国产日韩一区三区-成人激情毛片免费在线看-国产一区二区高清日韩-日韩成人黄片免费在线观看| 中文在线字幕亚洲精品-91麻豆天美精东蜜桃专区-黄色av电影免费在线观看-国产三级四级在线播放| 亚洲av男人的天堂久久精品-人妻中文字幕一区二区视频-国产男女乱淫真视频播放-国内人妻自拍交换在线视频| 日本一区二区三区乱在线视频-国产精品一区二区精品视频-日本人妻系列在线免费看-国产成人高清三级视频| 日本高清不卡码一区二区三区-国产性色av高清在线观看-亚洲黄色免费在线观看网站-亚洲性视频免费视频网站| 精国产精品亚洲二区在线观看-日韩人妻少妇一区二区三区-久久视频这里只要精品-亚洲精品欧洲综合在线观看| 日韩精品成人一区二区三区-亚洲综合中文字幕第一页-久久伊人亚洲中文字幕-花季传媒视频无限制观看| 亚洲av高清网站夜夜去-拍国产乱人伦偷精品视频-成人日韩欧美在线观看-无遮挡国产精品一级二级三级视频| 中文字幕在线精品人妻-人妻母乳综合一区二区三区四区-伊人久久婷婷色综合98网-亚洲人精品午夜射精日韩| 加勒比日本东京热风间由美-少妇高潮喷水高清av-国产免费观看久久黄av-永久成人免费在线视频| 国产在线观看av自拍-成人自拍小视频在线看-十八禁网站在线免费观看-丰满的熟妇露脸大屁股| 亚洲精品一区二区三区麻豆-国产精品小视频在线看-亚洲国产成人av第一二三区-国产不卡一区二区三区免费视频人| 青草青青视频精品在线-久热这里只有精品视频免费-免费av一级国产精品-尤物视频网站在线播放| 国产精彩自拍视频在线-岛国视频免费在线播放-91久久精品国产综合另类专区-午夜福利欧美激情福利| 免费观看一区二区av蜜桃-免费一级特黄久久大片-每日更新日韩中文字幕有码-97视频在线观看午夜| 91精品天堂福利在线观看漫画-亚洲国产精品一区亚洲国产-亚洲国产成人最新精品资源-亚洲国产精品成人综合久| 国产亚洲欧美日韩俺去啦-91香蕉国产极品在线播放-国产夫妻生活自拍视频-永久免费的成年视频网|