Dual-phase carbide refers to a type of carbide material that contains two different forms of grains. Typically, these two forms refer to plate-like grains and columnar grains. By adjusting the manufacturing process and parameters of the alloy, the proportion and arrangement of plate-like and columnar grains can be controlled. The preparation of dual-phase hard alloy can enhance the comprehensive performance of the alloy by combining the bending strength of plate-like grains with the uniformity of columnar grains, thereby improving the mechanical properties and service life of the hard alloy.

Brief history of WC carbide

Cemented carbide, born in 1923, emerged from a legendary and awe-inspiring nation – the Germanic people.

In the late 19th century, in search of new materials to replace high-speed steel and further enhance metal cutting speed, reduce processing costs, and solve issues like tungsten wire drawing for light bulbs, people began exploring the production of cemented carbide products.

In 1893, German scientists heated tungsten trioxide and sugar together in an electric furnace to high temperatures, successfully producing tungsten carbide. They attempted to utilize its high melting point and hardness to create wire drawing dies, as a substitute for diamond materials. Unfortunately, due to the brittleness, susceptibility to cracking, and low toughness of tungsten carbide, the first exploration of cemented carbide was declared a failure.

Entering the 1920s, German scientist Karl Schroter studied and discovered that pure tungsten carbide could not withstand the intense stress changes occurring during the drawing process. Only by adding low-melting-point metals to WC could the blanks possess a certain level of toughness without compromising hardness. Schroter proposed a method of powder metallurgy, mixing tungsten carbide with a small amount of ferrous metals (iron, nickel, cobalt), then pressing and sintering the mixture at temperatures exceeding a thousand degrees Celsius, resulting in the birth of the world’s first cemented carbide.

The continuous pursuit of cemented carbide with higher hardness and greater toughness led to the development of advanced production equipment for cemented carbide. In 2005, a team led by Professor Zhu Min from South China University of Technology in China introduced cold plasma into mechanical ball milling. By ball milling W, C, and Co powders with plasma, they were able to directly sinter the pressed green compacts into high-performance cemented carbide, achieving a one-step method for preparing high-performance and controllable W-C-Co cemented carbide.

 

The production of traditional hard alloys

The production process of traditional WC-Co cemented carbide is generally complex. It involves the reduction of tungsten oxide, carburization of tungsten, wet grinding of the mixed powders, drying and granulation of the mixed powders, compact pressing, debinding, and sintering. Clearly, this production process is intricate and has a relatively long production cycle. It also requires two high-temperature processes for carburization and sintering, resulting in high energy consumption, as shown in Figure

What is 2-phase WC Carbide? 2

fig1:The production of WC-Co carbide using traditional industrial methods

 

The utilization of low-temperature plasma-assisted high-energy ball milling (dielectric barrier discharge plasma-assisted milling, abbreviated as plasma milling) equipment has enabled the efficient refinement and activation of W-C-Co powders in a short period of time. Experimental results have confirmed that the composite powder obtained after discharge plasma milling (≤3 hours), when pressed and formed, can be directly sintered into WC-Co cemented carbide at around 1390°C, as shown in Figure 2.

What is 2-phase WC Carbide? 3

fig2:The one-step method for preparing WC-Co carbide, based on dielectric barrier discharge plasma-assisted milling technology

Compared to the traditional process of cemented carbide preparation, this method (carburization-sintering one-step method) avoids the drawbacks of the two high-temperature stages in the traditional process. It enables the synthesis of WC and the densification of WC-Co alloy bodies in a single step. This method is a new approach characterized by a short preparation process, simplified procedure, and low energy consumption. By utilizing this method and controlling the grain size and morphology of WC, as well as the arrangement state of plate-like WC, a novel high-performance cemented carbide with a dual morphology and dual-scale structure has been successfully prepared.

 

The one-step method for synthesizing carbide through carbide sintering

The one-step synthesis of cemented carbide is based on the discharge plasma-assisted ball milling technology. Firstly, the original W, C, and Co powders are subjected to plasma ball milling to produce nanocrystalline W-C-Co composite powder. The ball milling time is approximately 1-3 hours. Then, the prepared composite powder is cold pressed and formed into green compacts. Finally, the green compacts are carburized and sintered in a vacuum or low-pressure sintering furnace to obtain WC-Co cemented carbide bodies in a single step, as shown in Figure 2. The cemented carbide typically prepared by this method is a high-performance nanocrystalline or ultrafine-grained WC-8Co alloy.

What is 2-phase WC Carbide? 4

Figure 3 shows the DSC curves of W-C mixed powders milled for 3 hours using conventional ball milling and plasma-assisted ball milling. After plasma-assisted ball milling, the W-C mixed powder starts to form WC at around 900°C (the new plasma-assisted ball milling equipment can achieve WC synthesis below 800°C). This temperature reduction of 300-500°C compared to conventional carburization methods significantly shortens the carbonization process by tens to hundreds of hours compared to commonly used ball milling times.

What is 2-phase WC Carbide? 5

fig4:After 3 hours of plasma-assisted milling: (a) W-C powder; (b) morphology of W-C powder after sintering at 1000°C; (c) morphology of W-C powder after sintering at 1390°C.

It is highly meaningful that WC-8Co carbide prepared using the “one-step method” process exhibits excellent mechanical properties, as shown in Figure 5.

What is 2-phase WC Carbide? 6

fig5:The mechanical properties of WC-8Co carbide prepared by plasma-assisted milling with different scales

Based on the “carburization-sintering one-step method,” by adjusting the plasma ball milling time, it is possible to obtain cemented carbide with a combination of plate-like and prismatic WC in different proportions. When an appropriate proportion of plate-like and prismatic WC is achieved, the cemented carbide exhibits improved overall performance. This is because plate-like WC possesses good flexural strength, while the presence of prismatic WC effectively avoids the issue of lower transverse rupture strength (TRS) caused by highly oriented arrangement of plate-like WC on the cross-section.

The synergistic effect of the two different forms of WC ensures the uniformity of the mechanical properties of the cemented carbide and effectively enhances its comprehensive mechanical performance. For example, for WC-8Co cemented carbide prepared by vacuum or low-pressure sintering, when the percentage of plate-like WC is around 35%, its hardness is HRA92.1, and the transverse rupture strength (TRS) is approximately 3800 MPa.

Therefore, the development of the “carburization-sintering one-step method” for preparing WC-Co cemented carbide using plasma ball milling technology enables the microstructural control of WC in multiple forms and scales. This approach facilitates the production of high-hardness and high-strength WC-8Co cemented carbide.

 

High-performance dual-phase, dual-scale WC carbide

WC crystals belong to the hexagonal crystal system. The anisotropy of the hexagonal system results in different physical and mechanical properties of WC grains in each crystallographic direction or plane. The hardness of the WC (0001) basal plane is twice that of the WC (10-10) plane. When a certain amount of plate-like WC is present in cemented carbide and its distribution state is controlled by exploiting the anisotropy of plate-like WC grain properties, dual-phase cemented carbide with better performance than conventional cemented carbide can be prepared.

In the study of the effect of WC morphology on cemented carbide performance, it has been discovered that by carefully adjusting the plasma ball milling process, control of WC morphology as prismatic or plate-like (lamellar) can be achieved in the subsequent sintering process, as shown in Figure 6.

What is 2-phase WC Carbide? 7

fig6:Cold cylindrical and plate WC morphologies of different scales prepared by plasma ball grinding

Based on this foundation, the design and preparation of dual-phase cemented carbide with dual-phase WC grains have been achieved by adjusting the processing methods. The different morphologies of WC on different cross-sections demonstrate that the morphology of WC can be controlled to be either prismatic or plate-like by adjusting the ball milling time. In the study of the effect of plate-like WC content on improving mechanical properties, the proportion of different forms of WC in the cemented carbide matrix and the arrangement state of plate-like WC have been controlled through rational design.

Currently, while maintaining high hardness in the obtained WC-8Co cemented carbide, controllability in terms of strength has been achieved. The mechanical properties of the cemented carbide mainly include hardness = 91.5 ~ 93.0 HRA, TRS = 3300 ~ 4000 MPa, and KIC = 17.5 ~ 21.5 MPa*m1/2.

As shown in Figure 7, the content of different WC morphologies in a series of dual-phase cemented carbides and the mechanical properties listed in Table 1 indicate that the typical example C1P1 of dual-phase cemented carbide has a plate-like WC content of approximately 35%. The mechanical properties of the cemented carbide on different cross-sections are as follows: hardness on the cross-section = 92.4 HRA, TRS = 3795 MPa; hardness on the longitudinal section = 92.1, TRS = 3824 MPa. This indicates that the synergistic effect of the two different forms of WC not only ensures the uniformity of the mechanical properties of the cemented carbide on different cross-sections but also effectively improves its comprehensive mechanical performance.

What is 2-phase WC Carbide? 8

fig7:Variation in the content of columnar and lamellar WC in dual-phase WC carbide

What is 2-phase WC Carbide? 9

chart1:Hardness and TRS (tensile strength) of dual-phase WC-8Co carbide (corresponding to Figure 7).

In further research on the preparation of high-content plate-like WC cemented carbide, by selecting the particle size of the original tungsten (W) powder and employing a rational preparation process, the degree of orientation of plate-like WC can be well controlled, leading to a significant improvement in the transverse fracture strength of the cemented carbide, as shown in Figure 8.

What is 2-phase WC Carbide? 10

fig8:The process route for preparing dual-scale plate-like WC-Co carbide using plasma-assisted milling technology

In the current stage of research, the WC-8Co cemented carbide containing a high proportion of plate-like WC exhibits excellent mechanical properties, with the following optimal mechanical performance: cross-sectional hardness = 92.4 HRA, transverse rupture strength (TRS) = 4083 MPa, longitudinal hardness = 92.1 HRA, and TRS = 3924 MPa.

Schreibe einen Kommentar

Deine E-Mail-Adresse wird nicht ver?ffentlicht. Erforderliche Felder sind mit * markiert.

日本一区二区三区欧美精品-农村少妇真人毛片视频-亚洲av乱码专区国产乱码-跨年夜爆操极品翘臀日韩| 日韩一区二区三区视频在线观看-久久精品亚洲热综合一本色婷婷-国产亚洲精品视频一区二区三区-人妻中文字幕精品系列| 粉嫩精品一区二区三区在线观-中文国产精品久久久私一本-熟女少妇日韩亚洲av-精品国产一区二区三广区精东| 久久热大香蕉在线视频-nana在线观看高清视频 视频-久久最新视频在线观看-日韩高清不卡视频在线观看| 亚洲中文字幕中出在线-美女口爆吞精在线播放-亚洲欧美清纯唯美另类-国产一区二区三区免费观看不卡| 激情视频在线观看国产一区-日韩高清在线视频一区免费观看-国产白丝精品在线观看-色偷偷伊人大杳蕉综合网| 青草青青视频精品在线-久热这里只有精品视频免费-免费av一级国产精品-尤物视频网站在线播放| 精品视频在线观看免费一区二区-哪里可以看国产视频一区二区三区-亚洲天堂av在线免费观看-国产大片网站在线观看| 中文字幕在线精品人妻-人妻母乳综合一区二区三区四区-伊人久久婷婷色综合98网-亚洲人精品午夜射精日韩| 日韩成人深夜免费在线观看-成人av一区二区在线播放-日韩无套内射免费精品-国产精品一区白嫩在线观看| 亚洲综合精品一区二区在线-国产亚洲精品视频在线播放-国产精品经典三级免费观看-五月婷婷六月丁香视频| 国产精品毛片一区二区三-av蜜臀永久免费看片-三级国产美女搭讪视频-亚洲中文字幕在线观看一区二区| 日本一区二区三区黄色网-亚洲国产综合久久天堂-精品国产乱码久久蜜桃-欧美少妇精品在线观看| 日韩黄色精品中文视频-久久精品国产亚洲懂色-欧洲美女日韩精品视频-国产一区二区三区精品愉拍| 男女公园上摸下揉视频-日本精品视频一二区-激情久久综合久久人妻-伊人成人综合在线视频| 国色天香精品亚洲精品-日韩精品电影免费观看-亚洲精品中文字幕综合-成人午夜视频福利在线观看| 国产精品蜜桃久久一区二区-久久精品熟女亚洲av麻豆蜜臀-日本一区二区精品色超碰-伊人一区二区三区久久精品| av免费在线观看网站大全-日本av一区二区三区视频-国产精品日韩一区二区在线-亚洲av永久精品一区二区三区| 欧美日韩在线视频一区不卡-高清自拍最新国产精品-亚洲自偷精品视频自拍-日韩在线不卡中文字幕| 亚洲一区二区三区四区中文字幕-精品久久久久久蜜臀-国产传媒视频免费观看网站-国产三级在线观看一区二区| 亚洲天堂男人的天堂在线-亚洲激情欧美日韩在线-国产av剧情精品老熟女-色老头与人妻中文字幕视频| 加勒比大香蕉优优久久-国产av精品国语对白国产-亚洲一区二区免费日韩-国产一级内射无挡观看| 国产精品成久久久久久三级四虎-亚洲成人av在线高清-国产精品一区二区三区自拍-欧美午夜激情视频网站| 九九久久精品国产av-日本高清在线观看一区二区-精品熟女视频一区二区三区-亚洲欧洲成熟熟女妇专区乱| 第一亚洲自拍偷拍一区二区-国产精品成人一区二区不卡-中文字幕一区二区三区精品人妻-一区二区三区中文字幕在线播放| 人妻体内射精一区二区三区小视频-国产精品久久久久人人爽-日韩三级黄色一区二区三区-亚洲伊人色综合网收藏| 中出少妇中文字幕一区二区三区-九九久久精品国产亚洲-美女免费是黄的一区二区av-日本在线视频观看91| 日本三十四十五十路熟妇-国产一区二区三区蜜桃视频-蜜桃传媒第一区免费观看-来点刺激的视频日韩经典三级| 亚洲乱码中文字幕小综合-欧美亚洲国产精品一区二区-中文字幕人妻系列人妻有码中文-一区二区三区在线观看的视频| 亚洲精品色国语对白在线-黄片毛片av在线免费观看-久久精品有码av天堂-日韩一区二区三区高清视频| 久久精品亚洲精品毛片-国产精品白丝在线播放-日韩国产欧美综合第一页-亚洲三a免费观看网站| 午夜视频在线观看色诱-久久精品午夜福利视频-熟妇人妻av一区二区三区-一区二区三区中文字幕在线观看| 99热亚洲熟女少妇一区二区-久草福利免费在线视频观看-人妻丰满熟妇av一区二区-日韩高清亚洲一区二区| 亚洲伊人色综合网站亚洲伊人-香蕉久久国产超碰青草91-激情综合七月插插综合-亚洲一区二区三区夏目彩春| 日韩精品一区二区蜜桃免费视频-色综合视频一区二区三区-欧美一级黄片视频在线播放-国产精品视频一区二区色戒| 3p人妻一区二区三区-亚洲精品国产高清自拍-女同国产日韩精品在线-亚洲午夜国产激情福利网站| 日本av自拍偷拍视频-日韩精品人妻一区二区三区-看片福利国产午夜三级看片-在线观看视频最新信息好幫手| 欧亚久久日韩av久久综合-国产性感美女色诱视频-色噜噜人妻丝袜av先锋影院先-二次元中文字幕色在线| 亚洲免费看三级黄网站-日韩国产熟女免费精品老熟女视频-久青草视频免费在线播放-国产日韩精品久久一区二区| 日韩av不卡一区二区-国产白丝精品91久久-午夜福利理论片在线播放-国产粉饼哪个牌子好用| 免费蜜臀av一区二区三区人妻-亚洲熟女少妇精品久久-国产精品毛片免费观看-亚洲精品国产二区中文字幕|