色呦呦网址在线观看,久久久久久久久福利精品,国产欧美1区2区3区,国产日韩av一区二区在线

Abstract3D gel printing (3DGP) is a novel manufacturing technology that builds 3D components by depositing and gelling metal slurries layer by layer. Herein, a hydroxyethyl methacrylate (HEMA)-based slurry having a solid loading of 47-56 vol% WC-20Co was directly formed by 3DGP and then sintered in a vacuum oven. WC-20Co slurries exhibit suitable flow and shear thinning behavior, which is advantageous for the 3DGP forming process. The effects of 3DGP processing parameters (such as printing inner diameter and filling rate) on the surface roughness and dimensional accuracy of printing blanks were studied. The effects of solid loading on the rheological properties, sintering density, sintering density and mechanical properties of WC-20Co slurry were studied. The results show that the sample can be printed with good shape, with appropriate accuracy and uniform microstructure. Sintered samples have good shape retention and a uniform microstructure. The best sample density, hardness and transverse rupture strength were 13.55 g / cm3, HRA 87.7 and 2612.8 MPa, respectively. 3DGP has unique advantages in the near-net shaping of complex-shaped WC-20Co elements. 1. IntroductionWC-Co cemented carbide consists of hard WC particles embedded in a continuous Co matrix and is one of the most important metal matrix composites. They are now widely used as drilling and cutting tools, stamping dies, wear parts and other special parts. Due to the infusibility of WC particles, cemented carbides are usually produced using the powder metallurgy (PM) process in which liquid phase sintering of WC-Co powder compacts occurs. The product’s shape complexity is severely limited by the die structure. In addition, because of the high hardness and strength-toughness properties of WC-Co hardmetals, it is difficult to process WC-Co hardmetals. The use of traditional methods to prepare complex shaped carbide parts is a huge challenge.In recent years, the additive manufacturing (AM) technology suitable for manufacturing near-net shapes and complex parts has been developed and applied to the production of several metal materials such as stainless steel, titanium, titanium alloys, and aluminum alloys (SLM). Direct metal laser sintering (DMLS), electron beam melting (EBM), etc. are typical and mainstream technologies. Laser Engineering Network Forming (LENS) can produce complex shapes and almost completely dense parts. In these AM processes, the metal powder is selectively layered by a laser/electron beam layer by layer until the parts are built. However, there are few studies on the additive manufacturing of WC-Co hardmetals. First, WC-Co cemented carbide consists of WC particles and a Co matrix material, and the melting points of the two materials are very different. When the WC-Co powder is heated to the melting point of Co, the WC particles remain in the solid state; the powder is further heated and Co begins to evaporate. Partial melting will reduce the density of the product. To solve this problem, some researchers tried to add some binders, such as low melting point metals. Gu et al. Cu powder and WC-10Co powder were mixed at a weight ratio of 60:40, and samples of 50 mm×10 mm×9 mm were manufactured using DMLS. Due to the large amount of Cu, the relative density of this sample reached 94.3%. Second, these powder bed fusion technologies have certain requirements for the powder used. In the SLM and EBM processes, metal powders propagate through the rollers, while DMLS and LENS are usually equipped with a synchronous powder feeding system. In order to obtain a uniform and thin powder layer, both powder feed types require fine powder and spherical powder with good flowability. Commercially irregularly shaped WC-Co powder does not meet these requirements. In addition, laser/electron beam heating and cooling (ie, sintering process) is very fast. Only a few WC particles can dissolve into the liquid phase. Incomplete sintering may reduce product performance. Finally, the above techniques require high vacuum or inert gas protection systems, which are costly and involve the decarburization and evaporation of cobalt. Bear et al. found that there was not enough free carbon in the powdered feedstock to compensate for the carbon loss that occurred during the LENS process. Although the above techniques can produce many complex parts, they may not be suitable for the production of WC-Co hardmetals. In order to solve the limitations of the conventional methods and the problems of the above-mentioned AM technology in the production of WC-Co hardmetals, a new AM process called 3D Gel Printing (3DGP) was proposed. 3DGP combines gel injection molding with the fused deposition model (FDM) and has the ability to convert 3D models into 3D solids. Figure 1(a) shows our designed 3DGP device. Figure 1(b) shows an enlarged view of the extrusion and deposition system of the device. First, the designed 3D model is cut into a series of 2D slices. The powdered slurry in the organic monomer solution is then used as an "ink" and conveyed to the screw extruder of the 3D GP equipment under the specific pressure of the compressed air. At the same time, the initiator and catalyst are delivered to the same screw extruder in proportion. The materials are thoroughly mixed and extruded through a nozzle and then deposited on a printing platform. After a short period of time, the organic monomers are crosslinked and the solid powder is held in place by a three-dimensional crosslinked polymer. In this way, the slurry is selectively deposited layer by layer, which is consistent with each pre-constructed 2D slice of the 3D model. Finally, a three-dimensional structure green body is obtained. In order to avoid the collapse of the green during the printing process, the printing platform remains stationary, and the print head of the 3DGP device can move along the X, Y, and Z axes, which is different from the conventional FDM device. Similar to traditional FDM devices, the new device has the advantages of flexible molding, simple structure, and accurate control. After drying, the green body is degreased and sintered in a vacuum or atmospheric furnace.Figure 1 Schematic of 3DGP: (a) 3D gel-printing apparatus, (b) enlarged view of the extrusion and deposition system, (c) slurry filaments and (d) deposition of the sericin filaments.Gel casting has been used to produce various metal materials and ceramics, such as WC-8 wt%Co, 17-4PH stainless steel, high-temperature alloy, Al2O3, Si3N4, SiC and so on. This proves that a variety of material powders can be stably dispersed and suspended in the organic monomer solution, which means that 3DGP has great potential in forming many materials including metals, metal alloys, metal matrix composites and ceramics. The current demand for complex carbide parts is constantly increasing. WC-20Co is a typical cemented carbide. In this study, WC-20Co slurry was used as a printable ink, and the additive manufacturing of the WC-20Co component was studied by 3DGP. The purpose is to manufacture high density, high mechanical properties of WC-20Co composite parts, and to study the feasibility and practicality of 3DGP in the near net shaping of WC-Co hard alloy parts.2. Preparation2.1. WC-20Co slurry preparationCommercial WC powder having an average particle diameter of 2.7 μm and Co powder having an average particle diameter of 46.5 μm were used in this work. Figures 2(a) and (b) show the appearance of WC powder and Co powder, respectively. These raw materials were mixed using a ball-milling mixture having a WC to Co weight ratio of 80:20 and a cemented carbide ball mixed with a WC-20Co powder in a weight ratio of 5:1. Figure 2(c) shows the WC-20Co composite powder after grinding for 24 hours.Fig. 2 The morphology of the powder material: (a) WC powder, (b) Co powder and (c) WC-20Co composite powder.To prevent oxidation of cobalt, non-hydrogel systems were designed. Toluene and hydroxyethyl methacrylate (CH2=C(CH3)COOCH2CH2OH, HEMA) were chosen as solvents and organic monomers. Table 1 lists the gel systems used for WC-20Co slurries.Table 1. Chemical Reagent System for WC-20Co Slurry.Solvent organic monomer crosslinker dispersant initiator catalystToluene-Hydroxyethyl Methacrylate (HEMA) N,N’-Methylene Bis-Acrylamide Solsperse-6000 Benzoyl Peroxide (BPO) Dimethyl Aniline (TEMED)The reagents used in the experiment were all analytically pure.First, HEMA (monomer) and N,N’-methylene-bisacrylamide (crosslinker) were mixed at a weight ratio of 80:1 and then dissolved in toluene at a concentration of 50% by volume of HEMA to prepare a pretreatment. mixture. Next, slurries with different solid loadings were prepared by dispersing the WC-20Co powder into the premixed solution. The dispersant Solsperse-6000 (ICI Co. USA, non-toxic) was added simultaneously in a certain proportion. These WC-20Co suspensions were then ball milled for 2 hours to obtain a uniform slurry.2.2. 3D gel printing processThe above WC-20Co slurry was delivered to a 3D GP device under appropriate pressure. Three nozzles with inner diameters of 0.5, 0.6 and 0.7 mm are used herein. Table 2 lists the print conditions of the 3DGP process. Based on these printing parameters, taking a bevel cutter as an example, some rectangular samples were prepared and analyzed to determine the accuracy and surface condition of the 3DGP. After the 3D gel printing process, the green bodies were dried in a vacuum oven at 60° C. for 8 hours. The dried green body was degreased at 700° C. for 1 hour and finally sintered in a vacuum carbon tube furnace (vacuum<2 Pa) at 1360° C. for 1 hour.Table 2. Printing conditions for 3DGP.Numbering print conditionsNozzle diameter thick print speed1 0.50 mm 0.35 mm 28 mm/s2 0.60 mm 0.45 mm 28 mm/s3 0.70 mm 0.55 mm 28 mm/s2.3. measuringThe viscosity of the WC-20Co slurry was tested using an NDJ-79 rotary viscometer at 25°C. Thermogravimetric analysis (TGA) and differential thermal analysis (DTA) were used to study the thermal weight loss and decomposition kinetics of organic binders when the heating rate was 10 °C / min under high-purity argon flow. Archimedes’ principle was used to measure green density and sintered density. The laser scanning confocal microscope was used to observe the surface roughness, appearance and cross-sectional morphology of the 3DGP green body. The appearance of the WC-20Co powder and the microstructure of the green and sintered samples were observed by scanning electron microscopy. The hardness of the sintered samples was tested using a Rockwell hardness tester with a diamond cone and a 60 kg load. The bending test of sintered specimens cut into 5 mm x 5 mm x 35 mm was conducted by an electronic universal testing machine at a loading rate of 10 mm/min. Each set of reported data is based on attributes obtained from 3 to 5 samples.3. Results and discussion3.1. Rheological Behavior and Gelation Process of WC-20Co SlurryThe quality of the slurry depends on two key factors: solid loading and viscosity. FIG. 3 shows the effect of solid loading on the viscosity of WC-20Co slurry at a shear rate of 20 s ?1 . The viscosity of the slurry increases with solid loading. Unlike the viscosity requirements of gel injection molding (usually <1 Pa·s), higher viscosity (meaning higher solids content) can be used in the 3DGP process. The 3DGP paste does not need to be filled with a mold, but only needs to have a certain degree of fluidity (usually <3 Pa·s) so that it can be extruded through the nozzle. However, excessive viscosity may hinder the extrusion of WC-20Co paste. For example, a slurry with a solids content of 59 vol% is too viscous to be extruded. In this study, four different solid-loaded WC-20Co slurries were directly printed by 3DGP: 47, 50, 53 and 56 vol%.Figure 3. Effect of solid loading on the viscosity of WC-20Co paste.In addition, the WC-20Co slurry exhibits pseudoplastic fluid properties. As shown in Figure 4, as the shear rate increases, the viscosity of the WC-20Co slurry decreases significantly, indicating shear thinning behavior. This indicates that the WC-20Co slurry can flow at high shear rates caused by air pressure and agitation, and can be extruded at a specific pressure through a small diameter nozzle. Once the slurry is extruded and the shear force disappears, the slurry filaments maintain their shape rather than spread during a short idle time before solidification. This shear thinning characteristic is very favorable for the extrusion and deposition of WC-20Co slurries in the 3DGP process.Figure 4. Relationship between apparent viscosity and shear rate for WC-20Co slurry.There is an idle time between the addition of the catalyst dimethylaniline (TEMED) and the initiator benzoyl peroxide (BPO) and the onset of gelation (crosslink polymerization). Optimizing free time is a key point of 3DGP. In the correct idle time, the screw of the extrusion system can strongly stir the WC-20Co slurry, catalyst and initiator, and ensure that the crosslinking polymerization of the HEMA monomer occurs rapidly after extrusion and deposition of the slurry. Before printing the next layer, the previous layer of slurry should have sufficient strength so that the green body can retain its shape and withstand its own weight. Cross-linking polymerization of HEMA is an exothermic reaction, so custom instruments with a thermometer are used to help determine idle time. In our previous work, we found a significant impact on the reaction rate of the catalyst TEMED, the TEMED concentration was 10 mmol / L crosslinking reaction occurs when the stability. Unlike the remarkable effect of the catalyst, it is more convenient to optimize the idle time and the polymerization rate by adjusting the concentration of the initiator. Once added to the WC-20Co slurry, the initiator BPO decomposes into free radicals, successfully initiating the polymerization reaction. Figure 5 shows the effect of initiator concentration on the dead time of WC-20Co slurry with a solids content of 56% by volume. The results show that the gelation of the WC-20Co slurry is controllable. Idle time decreases with increasing initiator concentration. When the initiator concentration is 40 mmol / L, idle time is > 20 min. However, as the initiator concentration increased to 70 mmol/L, idle time decreased to about 5 minutes. When the concentration exceeds 100 mmol / L, the minimum idle time of impact. Similar patterns apply to slurries with different solids content. According to the results of repeated experiments presented initiator (90 mmol / L) of the optimum dosage. During this optimum unloaded period (about 2 minutes), the WC-20Co slurry was mixed with a certain amount of catalyst and initiator in a screw extruder and then extruded through a nozzle and finally cured in 20 seconds.Fig. 5 Effect of Initiator Concentration on the Empty Time of WC-20Co Slurry3.2. Characterization of Green BodyThe WC-20Co slurry was extruded through a conventional nozzle and due to the Barus effect (extruded expansion), the diameter of the slurry filament was slightly larger than the inner diameter of the nozzle. As shown in Fig. 1(c), after the slurry filament is deposited on the printing platform, its own gravity, rheological properties and slight contact with the nozzle will become semi-elliptical, as shown in Fig. 1(c). By controlling the idle time, the printing paste can be quickly cured and sufficiently strong before the next layer is extruded. Figure 1(d) is a schematic of the 3DGP deposition process. The WC-20Co slurry filaments are cross-stacked and the next layer will fill the void space of the previous layer. Due to the aforementioned Barus effect, it is necessary to choose the correct filling rate. The effect of fill rate is shown in Figure 6. Three different fill-rate samples were printed with a 0.7 mm nozzle and a WC-20Co paste with 56 vol% solids. When the filling rate is 100%, the WC-20Co slurry will pile up, deform, and then damage the shape of the product. On the other hand, as shown in the lattice structure shown in FIG. 6(a), the low filling rate results in a low density of the green body. With a filling rate of 92%, the green body formed well. The appropriate filling rate is selected based on the rheological properties of the slurry and nozzle size.Figure 6 Green samples with different filling rates: (a) 84%, (b) 92% and (c) 100%.The inner diameter of the nozzle affects the thickness of the deposited layer and ultimately determines the surface roughness and dimensional accuracy of the green body. To illustrate this, several samples were made by 3DGP using different diameter nozzles and WC-20Co slurry with 56 vol% solids loading. Their layer thickness, surface roughness, shape and size were measured to calculate the 3DGP forming accuracy. The layer thickness and surface roughness of the printed samples were studied by confocal laser scanning microscopy. FIG. 7 is a side view of a green body obtained by 3DGP using three nozzles with inner diameters of 0.5, 0.6, and 0.7 mm. This indicates that the slurry filaments maintain their shape and cure in time, with good bonding between layers. Table 3 shows the layer thickness, surface roughness and dimensions of the printed green body. The results of the measured layer thicknesses (0.355 mm, 0.447 mm and 0.552 mm, respectively) are consistent with the settings of the 3DGP shown in Table 2. As the nozzle diameter increases, the surface roughness of the printed sample increases. When a rectangular parallelepiped sample was printed using a nozzle with an inner diameter of 0.5 mm, a surface roughness (Ra) of 8.13±0.6 μm was obtained. When the inner diameter of the nozzle was increased to 0.7 mm, the sample had a surface roughness (Ra) as high as 19.98±0.9 μm. As can be seen from Table 3, all of these printed blanks are slightly larger than the three-dimensional model, but are slightly smaller during the drying process and are therefore closer to the model. Figure 8 shows a dried rectangular sample printed using a 0.5 mm nozzle and a WC-20Co slurry with a 56 vol% solids loading. As shown in Figure 8(b), the surface of the 3DGP-bulit sample had no obvious pores, splinters, and warpage defects. The line print marks are still visible on the surface of the cuboid sample. The results show that the 3DGP device has good forming ability, and the use of fine nozzles to prepare samples results in lower surface roughness and higher dimensional accuracy. Figure 8(e) shows a cross-section of a low magnification green dry sample. There is no interface between the print layer and the lines inside the green sample. Although the WC-Co paste is printed one by one layer by layer, the wetting and spreading properties of the paste are good, and the filling rate is appropriate, so that the wire and the layer have excellent adhesion. In addition, cross-linking polymerization of HEMA still occurs at these interfaces during the printing and drying steps and the tight bonding of the wires and layers. From the SEM image (Fig. 8(f)), it can be seen that the green sample has a uniform microstructure and the WC-Co particles are uniformly distributed. Moreover, the particles are tightly covered by the gel polymer and fixed in place.Figure 7: Side surface appearance and layer thickness of green bodies of different nozzles formed by 3DGP: 0.5mm nozzle, (b) 0.6mm nozzle, and (c) 0.7mm nozzle.Table 3. Layer thickness, surface roughness, and dimensions of the as-printed green bodies, and dimensions of dried green bodies. (The 3D model is 40 mm × 20 mm × 20 mm.)Fig. 8. The cuboid sample printed by 3DGP using 0.5 mm nozzle and WC-20Co slurry with a solid loading of 56 vol%: (a) three-dimensional model, (b) dried green body, (c) sintered sample, (e) cross section of dried green body under low magnification, and (f) microstructures of dried green body.Solid loading affects the density of the green body. As shown in FIG. 9, when a proper nozzle is selected and a proper filling rate is selected, the green density increases as the solid load of the slurry increases. At a solids load of 56 vol%, the green density was 7.85 g/cm3. The use of high solids content slurries facilitates the production of high density green compacts and reduces shrinkage during drying and sintering, which facilitates the achievement of high density homogenous and highly accurate sintered parts. In the premise of reasonable viscosity, it is necessary to increase the solid load as much as possible.Figure 9. Green density and sintered density of 3D GP samples with different WC-20Co solid loads.3.3. Sintered sampleThe 3DGP process is based on in situ polymerization of organic monomer binders and FDM. Prior to sintering, the green gel polymer (organic binder) should decompose and burn out. To investigate the thermal decomposition kinetics of organic binders, green samples printed using a WC-20Co slurry at 56 vol% solids loading were tested by TG and DTA in a flowing argon atmosphere at a heating rate of 10°C/min. . As shown in Figure 10, the green sample is endothermic due to the evaporation of toluene and becomes lighter at low temperatures (<100°C). The DTA curve shows a strong exotherm at about 450°C. Corresponding to the exothermic peak, the green body shows a significant weight loss between 300°C and 500°C. When heated to 600°C, the green sample lost 3.08 wt%. By calculation, the organic content of the dried green sample was 3.02% by weight. When the temperature is higher than 600°C, the weight of the green body hardly changes. The results show that the green polymer gel completely burned out after heating to about 600°C. Due to the low content of organic binders, 3DGP printed green samples only require thermal degreasing. 3DGP can form large-size components. The WC-20Co sample was annealed at 700° C. for one hour in consideration of the furnace temperature lag. In FIG. 8(c), it can be clearly observed that the shrinkage of the 3DGP-manufactured sample is uniform during sintering. The sintered sample maintains its shape without warping and has no defects on the surface.Figure 10. DTA curve and TG curve of a 3DGP sample with a heating rate of 10 °C/min.As the solid loading increases, the sintered density of the 3DGP sample increases. Just like the density data in FIG. 9, a sample printed using a WC-20Co slurry with a solids loading of 56 vol.-% showed a maximum density of 13.55 g/cm3, which reached 99.93% of the theoretical density. However, when the solid load was reduced to 47% by volume, the sintered density was only 12.01 g/cm 3 (88.58% of the theoretical density). The effect of solid loading is also reflected in the microstructure of the sintered sample. At a solid load of up to 56% by volume, the SEM image (Figure 11(a)) shows a sintered sample with near full densification with no cracks or voids observed. When the solid content is low, in other words, the solvent content and the organic binder content are high, the evaporation of the solvent and the burn-out of the organic binder cause many voids, which hinders sintering densification. FIG. 11(b) shows that when the solid loading of the WC-20Co slurry is reduced to 53% by volume, there are some small holes in the sintered sample. A large number of voids can be observed in FIG. 11(c) illustrating the microstructure of a sample printed using a WC-20Co slurry with a solids loading of 50% by volume. As shown in FIG. 11(d), more and more holes appear as the solid load is further reduced. There is not enough liquid phase during degreasing and sintering to fill the pores left by the solvent and organic binder. This resulted in low density and a large number of voids in the samples printed using WC-20Co paste with a solids loading of 47% by volume.Figure 11. (a) 56 vol%, (b) 53 vol%, (c) 50 vol%, and (d) 47 vol% WC-20Co slurry through a 3DGP printed SEM image of a sintered sample. Figure 12 shows the change in hardness of sintered samples as a function of WC-20Co slurry solid loading. At a solids loading of 47% by volume, the hardness (HRA) is only 84.5. Low solids content results in low sintered density (high porosity), which significantly reduces the mechanical properties of the sample. As the solid loading increases, the hardness increases significantly. Samples printed using a WC-20Co slurry having a 56 vol% solids loading have a maximum hardness (HRA) of 87.7.Figure 12. Hardness values of sintered samples with different WC-20Co solid loads.A similar situation occurs with the transverse rupture strength of the sintered sample. As shown in Figure 13, the flexural strength of the sample was observed to increase with increasing solid loading. The fracture appearance and microstructure of the sample (Figure 14) also confirmed this. As shown in FIGS. 14(b), (c) and (d), the sample had very low bending strength, and many holes were caused by low solid loads of 53%, 50%, and 47% by volume. Despite the presence of pores, it can be seen that the WC particles are uniformly distributed and no abnormal growth occurs. Samples made with a high WC-20Co content (56 vol%) slurry had a transverse rupture strength of 2612.8 MPa.Figure 13. Bending strength of sintered samples with different WC-20Co solid loads.Figure 14. Fracture patterns of WC-20Co samples printed using slurries with different solid loads: (a) 56 vol%, (b) 53 vol%, (c) 50 vol%, and (d) 47 vol%.Figure 15 shows a miter cutter (diameter 52 mm) made from 3DGP and sintered at 1360°C. Sintering shrinks evenly. Therefore, bevel milling has good shape retention. The mechanical properties of 3DGP printed samples are similar to the mechanical properties of samples made with conventional printing presses and sintering techniques. 3DGP is an advanced near net forming process that can form complex shapes without a mold (free forming). Printed lines can be viewed on a beveled surface. Parts made by 3DGP need to be polished and finished before use. The molding speed of 3DGP is still very slow. It takes 2 hours and 46 minutes to print bevel milling. As a non-molding process, 3DGP overcomes the limitations of complex shapes and simplifies the process flow. With the development of technology and equipment, forming accuracy and forming speed will gradually increase. 3DGP provides a new method for near net shaping of WC-Co hardmetal components.Figure 15. Bevelled cutter printed by 3DGP.4. conclusionThe composite WC-20Co component was successfully produced in a near net shape by a new AM process called 3D gel printing, which selectively deposits the WC-20Co slurry layer by layer. The following conclusions can be drawn:(1)Slurries with suitable rheological properties can be prepared using irregularly shaped WC-20Co composite powder and toluene-HEMA gel systems. Shear thinning behavior and controlled gelling reaction make WC-20Co slury suitable for 3DGP process.(2)3DGP can be used to make complex green bodies. The use of fine nozzles helps to improve the 3DGP’s forming accuracy and reduce the surface roughness of the sample. The packing rate should be selected based on the rheology of the slurry and the nozzle size. The printed sample has a good shape and a surface roughness of 8.13±0.6 μm. The low binder content of the greenware enables 3DGP to make large size components.(3)Increasing the solid loading of the WC-20Co slurry resulted in improvements in slurry viscosity, green density, sintered density, and mechanical properties of the sintered sample. The sintered sample printed using 56 vol% WC-20Co slurry has a density of 13.55 g/cm 3 (99.93% of theoretical density), hardness of 87.7 (HRA) and flexural strength of 2612.8 MPa. In addition, the microstructure is uniform with fine and uniform WC grains.Reference:Xin yue Zhang, Zhi, meng Guo ,Cun guang Chen, Wei wei Yang.Additive manufacturing of WC-20Co components by 3D gel-printing. International Journal of Refractory Metals and Hard Materials,Volume 70, January 2018, Pages 215-223
Source: Meeyou Carbide

Leave a Reply

Your email address will not be published. Required fields are marked *

日韩久久久久久中文字幕-九九热视频精选在线播放-亚洲最大黄色成人av-亚洲最大av一区二区| 日本一区二区三区欧美精品-农村少妇真人毛片视频-亚洲av乱码专区国产乱码-跨年夜爆操极品翘臀日韩| 欧美极品欧美精品欧美激情-人妻av中文字幕高清版-国产传媒麻豆天美在线观看-免费91麻豆精品国产自产自线| 追虎擒龙国语高清在线观看完整版-色婷婷一区二区三区免费-网友自拍在线视频国产-草草久在线视频在线观看| 国产传媒高清视频在线-日韩人妻少妇av在线-日本久久精品高清视频-丰满肥臀大屁股熟妇激情| 国内一级一厂片内射视频播放磨-国产乐播传媒在线观看-让你操水蜜桃在线观看-深夜三级视频在线观看| 亚洲一级特黄大片做受-国产91喷潮在线观看-日本不卡一区二区三区四区-在线观看高清视频一区二区三区| 国产精品 一区二区 久久-国产在线一区二区三区四区视频-午夜日本在线观看视频-日韩一区二区中文字幕18禁| 精品视频人妻少妇一区二区三区-人妻中文字幕一二三区-日本老熟妇成熟老妇人-东京热国产精品二区三区| 在线视频国产一区二区三区-亚洲欧美日韩国产经典-性插亚洲香蕉在线视频-亚洲成人国产超级黄色| 欧美性色婷婷久久久精品-久久这里只有精品国产宅男av-久久男女爱爱视频免费观看-另类福利亚洲丝袜激情在线| 国产午夜精品视频在线观看-亚洲欧洲日本元码高清-亚洲精品视频自拍成人-午夜福利欧美在线观看视频| 青青草视频在线观看免费网站-国产精品久久久久久亚洲影-在线播放国产精品一区二区-青青草免费观看高清视频| 日韩精品中文一区二区三区在线-午夜视频国产在线观看-日韩中文字幕av有码-最新日韩精品视频免费在线观看| 乱中年女人伦中文字幕久久-国产成人高清免费视频网站-中文字幕亚洲人妻在线视频-中文字幕剧情av在线| 亚洲av高清网站夜夜去-拍国产乱人伦偷精品视频-成人日韩欧美在线观看-无遮挡国产精品一级二级三级视频| 国产色悠悠综合在线观看-亚洲av综合av一区-久久久久国产精品三级网-欧美日韩精品一区二区不卡| 九九久久精品国产av-日本高清在线观看一区二区-精品熟女视频一区二区三区-亚洲欧洲成熟熟女妇专区乱| 国产大波精品一区二区在线-男女床上激情免费网站-日韩成人在线高清视频-国产精品视频免费自拍| 国产精品一区二区三区四区-日本毛茸茸的丰满熟妇-中文字幕久久中文字幕久久-国产成人三级一区二区在线观看| 欧美日韩激情片在线观看-色男人天堂网在线观看-亚洲一级特黄大片免色-国产十八禁免费在线观看| 中文字幕一区二区三区日韩精品-久久老熟女一区二区三区福利-久久精品国产自产对白一区-午夜欧美牲交激情网站| 亚洲不卡福利在线视频-亚洲一级特大黄色小视频-日本久久一级二级三级-国产精品剧情av在线观看| 九九热在线视频精品一-国产乱码精品一区二区蜜臀-乱妇乱熟女妇熟女网站视频-国产精品午夜视频在线| 不卡一区二区三区视频-国产亚洲91精品色在线观看-国产精品青草久久福利不卡-国产黄色免费精品网站| 亚洲黄色美女视频大全-成上人色爱av综合网-亚洲一区二区三区激情在线观看-久久91精品国产一区二区| 激情综合亚洲欧美调教-亚洲综合日韩精品国产-国产成人亚洲精品av大片-久草青青亚洲毛片在线视频| 国产偷拍自拍视频在线观看-丰满欧美熟妇视频在线-亚洲午夜激情在线观看-四虎视频精品免费观看| 美女福利视频一区二区-在线观看你懂的日韩精品亚洲-男女丁丁一进一出视频-蜜臀av一区二区三区精品人妻| 日韩精品一区二区三中文字幕-欧美亚洲日本精品一区二区-日韩av亚洲在线观看-亚洲欧美国产日韩激情| 四虎永久在线精品免费青青-久久久久久久 国内精品-国产精品四虎永久免费视频-男人天堂av免费观看| 亚洲人妻av在线播放-日韩午夜短视频在线观看-91精品久久午夜中文字幕-亚洲熟伦熟女新五十熟妇| 日本免费精品一区二区三区四区-天天日天天射天天综合-国产在线精品免费av-高潮一区二区三区久久亚洲| 女人毛茸茸的外阴视频-成人激情午夜福利视频-国产精品性色一区二区三区-国产中文字幕欧美激情| 草草草草伦理少妇高清-国内精品视频网站草草-国产精品精国产在线观看-国产麻豆激情av在线| 免费人成视频在线播放-成人级a爱看片免费观看-激情偷乱在线视频播放网-激情综合网激情综合网激情| 日韩中文有码字幕在线观看-黑人国产一区二区三区-久久国产精品久久精品-国产激情在线一区二区三区| 91精品18国产在线观看-午夜福利原创精品视频-欧美日韩在线亚洲另类-欧美日韩亚洲国产综合在线| 极品尤物在线免费观看-超碰九七精品在线观看-午夜爱爱免费观看视频-日本免费人成黄页在线| 3p人妻一区二区三区-亚洲精品国产高清自拍-女同国产日韩精品在线-亚洲午夜国产激情福利网站| 国产精品一线天粉嫩av-亚洲视频在线观看一区二区三-深夜男人福利在线观看-中文字幕国产精品第一页|