The performance of tool breakage

1) Cutting edge micro collapse

When the material structure, hardness and allowance of workpiece are not uniform, the front angle is too large, the cutting edge strength is low, the rigidity of the process system is insufficient to produce vibration, or intermittent cutting is carried out. If the grinding quality of the cutting edge is not good, the cutting edge is prone to micro collapse, that is, the edge area appears small collapse, notch or peeling. In this case, the tool will lose part of its cutting capacity, but it will continue to work. In the process of continuous cutting, the damaged part of the blade area may expand rapidly, leading to greater damage.

2) Chipping of cutting edge or tip

This kind of damage is often produced under the cutting conditions which is worse than the micro collapse of cutting edge, or the further development of micro collapse. The size and range of the broken tool are larger than that of the micro collapse, which makes the tool completely lose cutting ability and has to stop working. The case of a knife tip breaking is often called a tip drop.

3) Broken blade or tool

When the cutting conditions are extremely bad, the cutting amount is too large, there is impact load, and there is micro crack in the blade or tool material. When welding and grinding exist residual stress in the blade, and the operation is not careful, the blade or tool may break. After this kind of damage, the tool can not be used continuously, so it can be scrapped.

4) Blade surface peeling off

For materials with high brittleness, such as cemented carbide, ceramics, PCBN with high tic content, the surface layer is easy to peel off due to defects or potential cracks in the surface structure, or residual stress in the surface due to welding and edge grinding. The peeling may occur on the front surface, and the knife may occur on the back side. The peeling object is flaky and the peeling area is large. The possibility of coating tool peeling is high. After the blade is slightly peeled, it can continue to work, and the cutting ability will be lost after serious peeling.

5) Plastic deformation of cutting parts

Because of the low strength and low hardness, plastic deformation may occur in the cutting parts of the steel and high speed steel. When the cemented carbide works directly at high temperature and three-way compressive stress, the surface plastic flow will also occur, even the plastic deformation surface of cutting edge or cutting edge will collapse. Collapse usually occurs when cutting amount is large and hard material is processed. The elastic modulus of TiC based cemented carbide is smaller than that of WC based cemented carbide, so the former has faster plastic deformation resistance or failure. The plastic deformation of PCD and PCBN will not occur.

6) Hot crack of blade

When the tool is subjected to alternating mechanical and thermal loads, the surface of the cutting part will inevitably produce alternating thermal stress due to repeated thermal expansion and contraction, which will cause the blade to crack due to fatigue. For example, when the carbide milling cutter is in high speed milling, the teeth are constantly subjected to periodic impact and alternating thermal stress, and the comb cracks appear on the front face. Although some tools do not have obvious alternating load and alternating stress, because of the temperature of surface and inner layer is inconsistent, thermal stress will also be generated. In addition, there are inevitable defects in the inner part of tool materials, so the blade may also produce cracks. Sometimes the tool can continue to work for a while after the crack is formed, sometimes the rapid crack growth causes the blade to break or the blade surface is seriously flaking.

What Cause Risks of Unexpected Breakage on Maching Tool? 1

Tool wearing

according to the reasons for wear, it can be divided into:

1) Abrasive wear

There are some very hard particles in the processed materials, which can draw grooves on the surface of the tool, which is abrasive grinding damage. Abrasive wear exists on all sides, and the front surface is the most obvious. But for low speed cutting, the wear of hemp is not obvious because of the low cutting temperature, so abrasive wear is the main reason. The lower the hardness of the other tool, the more serious the abrasive hemp damage.

2) Cold welding wear

During cutting, there is a great pressure and strong friction between the workpiece, cutting and front and rear cutter surface, so cold welding will occur. Because of the relative movement between friction pairs, the cold welding will produce fracture and be taken away by one side, which will cause the cold welding wear. The wear of cold welding is usually serious at medium cutting speed. The results show that brittle metal has better cold welding resistance than plastic metal; The multiphase metal is smaller than that of one-way metal; The tendency of metal compound is smaller than that of single cold welding; The cold welding tendency of group B and iron in the periodic table of chemical elements is small. The cold welding of high speed steel and cemented carbide is serious when cutting at low speed.

3) Diffusion wear

In the process of cutting and contact between workpiece and tool at high temperature, the chemical elements of both sides spread in solid state, which changed the composition structure of the tool, made the surface of the tool vulnerable and intensified the wear of the tool. The diffusion phenomenon always keeps the object with high depth gradient continuously spreading to the object with low depth gradient. For example, cobalt in cemented carbide will rapidly spread to chip and workpiece at 800 ℃, and WC is decomposed into tungsten and carbon to steel; When the cutting temperature of PCD tool is higher than 800 ℃, the carbon atoms in PCD will transfer to the workpiece surface with a great diffusion strength, and the tool surface will be graphitized. The diffusion of cobalt and tungsten is serious, and the diffusion resistance of titanium, tantalum and niobium is strong. Therefore, YT cemented carbide has good wear resistance. When the temperature of ceramic and PCBN is as high as 1000 ℃ -1300 ℃, diffusion wear is not significant. Because of the same material, the workpiece, chip and tool will generate thermal potential in the contact area during cutting. This thermoelectric potential can promote diffusion and accelerate the wear of the tool. This kind of diffusion wear under the action of thermoelectric potential is called “thermoelectric wear”.

4) Oxidation wear

When the temperature increases, the surface oxidation of the tool produces soft oxide, which is caused by chip friction, which is called oxidation wear. For example, oxygen in the gas at 700 ℃ ~800 ℃ reacts with cobalt, carbide and titanium carbide in cemented carbide to form soft oxides; The chemical reaction of PCBN with water vapor at 1000 ℃

according to the wear form, it can be divided into:

Front face damage

When cutting plastic materials at a large speed, the front cutting surface near the cutting force will wear into crescent denture under the action of chip cutting, so it is also called crescent groove wear. In the early stage of wear, the front angle of the tool increases, which improves the cutting conditions and is conducive to the curl and fracture of the chip. However, when the crescent groove is further increased, the cutting edge strength is greatly weakened, which may eventually cause the breakage and damage of the cutting edge. When cutting brittle materials, or cutting plastic materials with lower cutting speed and thinner cutting thickness, crescent wear will not occur.

Wear of the blade tip

The wear of the tip is the wear on the back surface of the arc of the tip and the adjacent back side of the tool. It is the continuation of the wear on the back blade surface of the tool. Because of the poor heat dissipation conditions and stress concentration, the wear speed is faster than the back blade surface. Sometimes a series of grooves with spacing equal to the feed amount will be formed on the back of the pair cutter surface, which is called groove wear. They are mainly caused by the hardened layer and cutting pattern of the machined surface. When cutting hard cutting materials with a large hardening tendency, the groove wear is the most likely. The wear of the tool tip has the greatest influence on the surface roughness and machining accuracy of the workpiece.

Wear of rear cutter surface

When cutting plastic materials with large cutting thickness, the back face of the tool may not contact the workpiece due to the presence of chip lumps. In addition, the back face usually contacts the workpiece, and a wear belt with a rear angle of 0 is formed on the back surface. Generally, in the middle of the working length of the cutting edge, the wear of the back face is even, so the wear degree of the back face can be measured by VB of the width of the wear belt of the back cutting edge. Because the wear of various types of tools almost occurs in different cutting conditions, especially when cutting brittle materials or cutting plastic materials with a small cutting thickness, the wear of the tool is mainly the back surface wear, and the measurement of the width VB of the wear belt is relatively simple, so VB is usually used to represent the wear degree of the tool. The larger VB, not only increases the cutting force, causes the cutting vibration, but also affects the wear of the arc of the tool tip, thus affecting the machining accuracy and the surface quality.

What Cause Risks of Unexpected Breakage on Maching Tool? 2

methods for preventing the tool from being damaged

1) According to the characteristics of the processed materials and parts, the various types and brands of the tool materials are selected reasonably. Under the premise of certain hardness and wear resistance, the necessary toughness of the tool material must be ensured;

2) The geometric parameters of the tool are selected reasonably. By adjusting the front and rear angles, the main and secondary deflection angles, the blade inclination angle and other angles;

Ensure that the cutting edge and the cutting edge have good strength. Grinding out the negative chamfering on the cutting edge is an effective measure to prevent the tool from falling;

3) Ensure the quality of welding and grinding, and avoid defects caused by poor welding and edge grinding. The tool used in key process shall be grinded to improve the surface quality and check for cracks;

4) The cutting amount should be selected reasonably to avoid excessive cutting force and too high cutting temperature, so as to prevent the tool from being damaged;

5) The process system is as rigid as possible and vibration can be reduced;

6) Take correct operation method to avoid or reduce sudden load of tool.

What Cause Risks of Unexpected Breakage on Maching Tool? 3

The cause and Countermeasure of tool breakage

1) The blade brand and specification are not selected properly, such as the thickness of the blade is too thin or the brand is too hard and brittle when rough processing.

Countermeasures:

The brand with high bending strength and toughness is selected to increase the thickness of the blade or install the blade vertically.

2) The tool geometry parameters are not selected properly (such as too large front and rear angles).

Countermeasures:

The tool can be redesigned from the following aspects.

① Reduce the front and rear corners properly.

② The larger negative blade angle is adopted.

③ Decrease the main deflection angle.

④ Adopt larger negative chamfering or edge arc.

⑤ Repair and grind the transition cutting edge to enhance the cutting edge.

3) The welding process of blade is incorrect, which causes excessive welding stress or welding crack.

Countermeasures:

① Avoid the use of three-sided closed blade groove structure.

② Solder is selected correctly.

③ Avoid heating welding with oxyacetylene flame and keep it warm after welding to eliminate internal stress.

④ Use mechanical clamping structure as much as possible

4) The grinding stress and crack are caused by improper grinding method; The vibration of the teeth after grinding the PCBN milling cutter is too large, which makes the load of individual teeth too heavy, and also causes the tool beating.

Countermeasures:

① The grinding is performed by intermittent grinding or diamond grinding wheel.

② Soft grinding wheel is selected and the grinding wheel is kept sharp.

③ Pay attention to the quality of the grinding and strictly control the vibration and swing of the cutter teeth.

5) Unreasonable cutting quantity selection, such as too much, the machine tool is boring; When cutting intermittently, the cutting speed is too high, the feed is too large, and the blank allowance is not uniform, the cutting depth is too small; When cutting materials with high hardness tendency, such as high manganese steel, the feed rate is too small.

Countermeasures:

Re select the cutting amount.

6) The reasons of the uneven bottom surface of the cutting groove or the long extension of the blade are the reasons of the mechanical clamping tool.

Countermeasures:

① Trim the bottom of the knife groove.

② The position of cutting fluid nozzle should be arranged reasonably.

③ The hardened cutter rod adds cemented carbide gasket under the blade.

7) Excessive tool wear.

Countermeasures:

Change the cutting edge or change the cutting edge in time.

8) The cutting fluid flow is insufficient or the filling method is incorrect, which causes the blade to burst hot and crack.

Countermeasures:

① Increase the flow of cutting fluid.

② The position of cutting fluid nozzle should be arranged reasonably.

  1. Effective cooling methods such as spray cooling are used to improve the cooling effect.

④ The * cutting is used to reduce the impact on the blade.

9) The tool is not installed correctly, such as: the cutting tool is too high or too low; The end milling cutter adopts asymmetric milling.

Countermeasures:

Refit the tool.

10) The rigidity of the process system is too poor, which causes too much vibration of cutting.

Countermeasures:

① Increase the auxiliary support of the workpiece and improve the clamping rigidity of the workpiece.

② Reduce the overhang length of the tool.

③ Reduce the back angle of the tool properly.

④ Other vibration suppression measures shall be adopted.

11) Improper operation, such as: tool cut in from the middle of the workpiece, too strong action; Stop before you have returned the knife.

Countermeasures:

Pay attention to the operation method.

4、 Chip tumor

1) Causes of formation

In the part near the cutting edge, the contact area of the cutter chip is very high, so that the bottom metal of the chip is embedded in the micro uneven peak valley on the front cutter surface, forming a real metal contact without gap and thus the bonding phenomenon occurs. This part of the knife chip contact area is called the bonding area. In the bonding area, a thin layer of metal material will be deposited on the front cutting surface at the bottom of the chip. The metal materials of this part of the chip have undergone severe deformation and strengthened at the appropriate cutting temperature. With the continuous outflow of chips, the stagnant material will slip away from the upper layer of chip, which is the basis of chip tumor. Then, a second layer of stagnant cutting material will be formed on it, which will form debris deposits.

2) Characteristics and influence on cutting

① The hardness is 1.5-2.0 times higher than that of the workpiece material, which can replace the front tool surface for cutting. It can protect the cutting edge and reduce the front tool surface wear. However, debris flowing through the contact area of the tool workpiece will cause the back face wear of the tool.

② The working angle of the tool increases after the chip forming, which plays an active role in reducing the chip deformation and cutting force.

③ Because the chip lumps protrude outside the cutting edge, the actual cutting depth increases, which affects the dimension accuracy of the workpiece.

④ The chip deposit will cause “ploughing” phenomenon on the surface of the workpiece, which will affect the surface roughness of the workpiece. ⑤ The debris of the chip tumor will bond or embed into the surface of the workpiece, which will cause hard points, which will affect the quality of the machined surface.

From the above analysis, it can be seen that chip accumulating tumor is unfavorable to cutting and finishing.

3) Control measures

The following measures can be taken to avoid the chip tumor without binding or deformation strengthening between the bottom material and the front cutting surface.

① Reduce the roughness of the front cutter surface.

② Increase the front angle of the tool.

③ Reduce the cutting thickness.

④ Low speed cutting or high-speed cutting is adopted to avoid cutting speed which is easy to form chip forming.

⑤ The hardness and plasticity of the workpiece materials are improved by proper heat treatment.

⑥ The cutting fluid with good anti adhesion property (such as extremely pressure cutting fluid with sulfur and chlorine) is adopted.

???? ???????

?? ??? ??? ????? ????? ??????????. ?????? ????????? ???? ????? ?? *

国产av一区二区三区在线-亚洲国产欧洲在线观看-跪求能看的国产熟女av网-国内色精品视频在线网址| 青青草视频成人在线公开-激情中文字幕一区二区三区-亚洲国产精品综合久久网各-日本中文字幕有码高清| 亚洲熟女少妇av麻豆-男人一天堂精品国产乱码-欧美精品高清在线播放-亚洲国产午夜福利精品| 亚洲视频一区二区久久-亚洲欧美日韩精品中文乱码-亚洲尤物在线视频观看-欧美熟妇视频一区二区三区| 国产一区二区三区精品视频导航-精品国产av网站大全-男女草逼视频网站大全-国内成人在线激情视频| 自拍成人免费在线视频-91在线高清视频播放-国产美女口爆吞精系列-午夜福利黄片在线观看| 国产精品内射在线免费看-99久久国产精品一区二区三区-久久国产精品午夜福利-亚洲av精品一区二区三区| 少妇被搞高潮在线免费观看-亚洲av成人精品小宵虎南-日韩性生活免费看视频-日韩黄色大片在线播放| 午夜精品福利激情视频-婷婷国产五月天网久久精品-国产av麻豆嫩草视频-av日本中文字幕在线| 日本a亚洲中文字幕永远-美女极度色诱视频国产-国产熟女另类激情在线-高潮少妇高潮少妇av| 无套进入极品美女少妇-新久久久高清黄色国产-国产肥臀在线精品一区二区-深夜午夜福利在线观看| 成人精品一区二区三区不卡-十八禁啪啪啪一区二区三区-后入黑丝美女在线观看-国产熟女啪啪免费视频| 亚洲av成人午夜福利在线观看-日韩精品成人影院久久久-国产在线高清不卡一区-激情五月另类综合视频| 日韩久久久久久中文字幕-九九热视频精选在线播放-亚洲最大黄色成人av-亚洲最大av一区二区| 国产精品乱码一区二区三区视频-国产自拍精品在线一区二区-五月综合丁香婷婷久久-在线国产精品一区二区三区| 91精品在线播放黑丝-在线观看精品国产自拍-av免费在线播放日韩-日韩av在线精品一区二区三区| 一本色道亚州综合久久精品-91麻豆国产专区在线观看-一级二级三级国产视频-熟女av天堂免费高清| 国产美女高潮久久精品-国产成人精品十八禁在线播放-成在线人视频免费视频-97超级视频在线观看| 欧美日韩偷拍丝袜美女二区-精品少妇人妻av免费久久洗澡-四虎精品永久在线观看视频-亚洲国产成人一区二区在线观看| 日韩视频精品在线播放-国产91亚洲精品久久-亚欧洲乱码视频在线观看-亚洲国产成人91精品| 免费手机在线观看bbb视频-国产欧美亚洲精品第1页青草-国产黄a三级三18级三级看三级-宅男视频在线观看一区二区三区| 加勒比大香蕉优优久久-国产av精品国语对白国产-亚洲一区二区免费日韩-国产一级内射无挡观看| av成人在线免费观看-亚洲av黄片免费观看-亚洲综合精品天堂夜夜-久久国产精品久久国产精品| 亚洲自拍偷拍另类第一页-麻豆国产午夜在线精品-久久精品一区二区三区综合-日本最近中文字幕免费| 亚洲国产高清一区二区三区不卡-亚洲综合小综合中文字幕-亚洲黄色成人av在线-日韩一区二区三区av观看| 超碰国产传媒在线观看-av在线免费观看蜜臀-亚洲欧美国产一区二区综合-人妻久久精品夜夜爽一区二区| 91九色国产成人久久精品-亚洲av无一区二区三区av中文-最新日本加勒比在线视频-激情综合激情五月婷婷| 午夜性色福利在线视频福利-久久精品视频免费获取地址-亚洲一区二区三区在线观看不卡-无套进入美女免费观看视频| 亚洲视频第一页在线观看-最新中文字幕国产精品-中文人妻熟妇人伦精品熟妇-国产福利91在线视频| 蜜桃视频大全免费观看-国产高清不卡一区二区-亚洲av综合av东京热三区-无套内射激情国产av| 日韩有码中文在线视频-少妇我被躁爽到高潮在线观看-精品丰满人妻一区二区三区-亚洲天堂高清在线播放| 亚洲乱码中文字幕小综合-欧美亚洲国产精品一区二区-中文字幕人妻系列人妻有码中文-一区二区三区在线观看的视频| 99热久久热在线视频-久久精品国产亚洲av成人男男-国产精品日韩精品久久99-中文字幕在线日本乱码| 乱女乱妇熟女熟妇综合网-亚洲都市激情中文字幕-日韩精品中文字幕在线-在线观看国产中出白浆| 国产一区二区三区在线播放-偷拍女厕尿尿在线免费看-午夜一区二区三区三区-国产精品一区二区三上人妻| 国产在线精品一区二区中文-亚洲小说欧美另类激情-97碰久日韩视频在线观看-日本一道本高清不卡区| 精品国产亚洲av蜜臀-欧美亚洲伦理在线视频-久久亚洲国产成人影院av-国产精品99蜜臀久久不卡二区| 国产精品一二三四区无线乱码-精品亚洲国产成人精品-国产精品蜜桃一区二区三区-黄片av在线免费播放| 亚洲不卡视频一区二区三区-99久久精品国产成人综合-国内精品熟女亚洲精品熟女-亚洲日本成人在线观看高清| 亚洲天堂av中文在线-亚洲精品有码中文字幕网络-在线播放国产一区二区不卡-香港毛片免费观看视频| 中文字幕亚洲天堂第一页-国产午夜福利在线视频-亚洲精品中文字幕女同-亚日韩精品一区二区三区|