Carbide sealing rings are usually made of WC-Ni carbide, due to its high hardness, bending strength, excellent wear resistance, toughness, and rigidity, does not emit radiation under neutron irradiation. As a result, it can be employed for mechanical sealing in conditions involving high temperature, high pressure, high rotational speeds, corros ive media, solid particle-laden media, and radioactive environments. WC-Ni carbide has found extensive application in fields such as axle seals in vehicle transmission systems, power shift transmissions, specialized pumps for demanding conditions, aircraft rotary seals, petrochemical industries, and nuclear power sealing.

We found that after approximately 80 hours of operation, there were numerous cracks on sealing rings’surface. Continuing to use it could lead to seal failure and result in significant economic losses. Therefore, it is necessary to conduct damage analysis and safety assessment to address this issue.

 

Test Materials and Methods

Test Materials

The test specimens were taken from the WC-Ni carbidesealing ring, designated as YWN8. The inner diameter of the sealing ring is 277 mm, the outer diameter is 302 mm, and the thickness is 20 mm, as shown in Figure 1. The primary material of the sealing ring is WC-Ni carbide, with a WC mass fraction of 89% and a Ni mass fraction of 11%. The mechanical properties of the WC-Ni carbide?are presented in Table 1.

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 1

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 2

Test method

Figure 1(a) depicts a solid view of the damaged sealing ring, which features 9 sets of groove weirs/barricades structures. As indicated by the labels 1 to 9 in Figure 1(b), the test is organized based on the distribution of groove weir areas in the sealing ring, dividing them into 9 groups. Further, these 9 groups are subdivided into 18 smaller regions. Upon magnified observation using a microscope, it was observed that 6 of these regions exhibited surface cracks: namely, 2-2, 3-2, 4-2, 5-2, 6-2, and 7-2, whereas the remaining regions showed no cracks on their surfaces.

For analysis, the test selected the areas of the damaged sealing ring where cracks appeared on the sealing surface. Subsequent steps involved surface residual stress testing, microscopic analysis of the damaged sealing ring’s microstructure, and identifying the reasons behind the appearance of cracks on the sealing ring’s surface.

 

Results and Analysis

Microscopic Analysis of the Damaged Area

Based on microscopic observations, the 6-2 damaged region exhibited the highest number of cracks. As shown in Figure 2, the SEM morphology of the 6-2 damaged region specimen reveals that there are a total of 5 cracks in the damaged zone. The origins of these cracks are at the junction between the groove weir and the barricade of the sealing ring. Each crack exhibits a trend of expansion along its length.

sealing ring

Analysis Using White Light Interferometer

Based on the SEM analysis mentioned above, it was found that although the crack volume was significant, the cracking depth was relatively shallow. To further investigate the damage characteristics during the sealing ring’s service, white light interferometry (Bruker Contour GT 3D white light interferometer) testing and analysis were performed on the damaged area of the sealing ring.

Figures 3 and 4 respectively depict the three-dimensional morphology at the location of the largest crack and the two-dimensional profile of the deepest point of the crack in the 6-2 damaged region. The results reveal that the roughness of the groove weir area is approximately 0.672 μm, the roughness of the barricade area is about 0.294 μm, and the height difference between the groove weir area and the barricade area is approximately 2.43 μm. The maximum width of the crack is around 126.4 μm, with a maximum length of about 2.75 mm. During testing, the maximum depth of the crack was found to be around 58.84 μm, while the depths of other crack regions were relatively smaller.

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 3

Chemical Composition Analysis of the Damaged Area

Energy-Dispersive X-ray Spectroscopy (EDS) Analysis

Based on the microscopic morphology analysis of the mentioned cracks, energy-dispersive X-ray spectroscopy (EDS) was used to analyze the chemical composition of points A, B, and C (corresponding to the specimen matrix, crack area, and the boundary strip between the groove weir and the barricade) as indicated in Figure 2. This was done to determine whether there had been any changes in material composition. The results are shown in Figures 5 to 7.

It can be observed that the specimen matrix primarily contains C, O, Ni, and W. In the crack area, in addition to the aforementioned four main elements, there are also impurity elements such as Cu, Fe, and Ti. This suggests that element transitions occurred in the sealing ring’s mating parts during service, resulting in impurity elements on its surface. The oxygen content in the crack area is significantly higher than that in the matrix, indicating the presence of oxides within the crack area and the occurrence of oxidative wear. Similarly, at the boundary strip between the groove weir and the barricade, in addition to the four main matrix elements, there are trace amounts of impurity elements such as Ti, Fe, and Zr. The damage situation here is similar to the crack area, with the presence of oxidative wear phenomena.

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 4

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 5

Electron Probe Microanalysis (EPMA) Analysis

To further investigate the extent of damage to the sealing ring and the characteristics of the cracked area, and to analyze the distribution of chemical composition in the damaged area of the sealing ring, electron probe microanalysis (EPMA) was employed to perform surface analysis on the cracked area within the box shown in Figure 8. Based on the EDS analysis results mentioned above, it was established that oxidative wear occurred during the service of the sealing ring. Therefore, four elements—C, W, Ni, and O—were selected for EPMA surface analysis of the test specimen.

Figure 9 presents the EPMA surface analysis results of the specimen. It can be observed that within the cracked area, there is a relatively higher distribution of C and O compared to the matrix, while the distribution of W within the cracked area is relatively lower compared to the matrix. On the other hand, the distribution of Ni within the cracked area does not exhibit significant differences compared to the matrix. It can be inferred that there is a mild level of oxidation within the cracked area, with the primary oxidation product being oxide of W.

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 6

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 7

Surface Residual Stress Analysis

To investigate the surface stress distribution of the sealing ring after service, a portable X-ray residual stress tester was used to conduct residual stress testing on the entire end face of both an unused C# sealing ring and a D# sealing ring (with cracks on the surface) that had been in service for 80 hours. The test positions and their results are shown in Figure 10. It can be observed that unevenly distributed surface residual stress can lead to cracks in the sealing ring. During service, residual stress is released due to friction, resulting in crack formation and failure of the sealing ring.

As shown in Figure 11, the residual stress gradually decreases along the radial direction of the sealing ring from the outer ring to the inner ring, transitioning directly into compressive stress in the barricade area. The stress value at the end of the groove weir area is higher than at the beginning (counter-clockwise along the sealing ring). Observed cracks are all located at the end of the groove weir area, indicating that the stress difference between the beginning and end of this area is relatively low compared to the stress difference between the arc ends. This difference in stress is insufficient to cause damage to the sealing ring.

 

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 8

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 9

 

 

 

Conclusion

(1) The majority of crack sources are located at the junction between the groove weir and the barricade of the sealing ring. Most cracks are distributed in the barricade area, where the extent of damage is greater compared to the groove weir area.

(2) Oxidative wear occurred in the damaged area of the sealing ring during service, primarily resulting in oxide products of tungsten (W). The oxidation is relatively mild.

(3) Due to a significant stress difference between the groove weir and the barricade areas of the sealing ring, material damage is prone to occur during service, leading to the initiation of microscopic cracks.

(4) The cracks are relatively shallow, and the damage to the sealing ring is minor. This will not have an immediate impact on operational safety within the short term.

How is?the Metal?Damage on?Carbide?Sealing Ring Formed? 10

 

 

 

 

Leave a Reply

Your email address will not be published. Required fields are marked *

少妇人妻午夜精品视频-亚洲乱妇老熟女爽到潮的片-最新国产黄色一区二区-亚洲一区国产精品喷潮| 91国自产区一二三区-日韩高清不卡一区二区三区四区-免费欢看欧美黄色国产-成人无遮挡毛片免费看| 18禁无遮挡美女国产-久久精品国产精品亚洲毛片-国内精品极品在线视频看看-日本二区 欧美 亚洲 国产| 密臀av免费在线观看-日韩欧美中文字幕美利坚-av黄色在线观看一区二区三区-日韩性做爰片免费视频看| 久久国产精品亚洲va麻豆-嫩模大尺度偷拍在线视频-免费三级在线观看自拍-天堂av在线男女av| 久久精品国产亚洲av麻豆看片-内射后入高潮在线视频-亚洲精品一区三区三区在线-亚洲乱码一区二区三区视色| 精品人妻中文字幕有码在线-亚洲欧美一区二区成人精品久久久-亚洲第一人伊狼人久久-亚洲国产欧美精品在线观看| 亚洲一区二区三区日本久久-精品国产成人一区二区不卡在线-91精品国产色综合久久成人-一区二区三区成人在线观看| 国产一区二区在线中文字幕-欧洲中文字幕国产精品-国产精品蜜臀av免费观看四虎-国产一级特黄99久久| 国产91精品一区二区亚洲-国产精品国产三级国产播-久久国产精品免费一区六九堂-五月婷婷六月丁香激情网| 91久久国产综合蜜桃-深夜激情在线免费观看-免费观看国产在线视频不卡-天堂在线精品免费亚洲| 九九热在线免费视频播放-久久综合九色综合久久久-国产粉嫩小仙女裸体区一区二-中文字幕巨乳人妻在线| 日本一区二区三区四区高清-91久久香蕉国产熟女-久久精品99国产日本精品-国产粉嫩一区二区三区在线观看| 第一亚洲自拍偷拍一区二区-国产精品成人一区二区不卡-中文字幕一区二区三区精品人妻-一区二区三区中文字幕在线播放| 2020天天操夜夜操-亚洲色图视频在线观看,-亚洲色图专区另类在线激情视频-岛国精品毛片在线观看| 欧美性色婷婷久久久精品-久久这里只有精品国产宅男av-久久男女爱爱视频免费观看-另类福利亚洲丝袜激情在线| 国产二区三区视频在线观看-四虎精品一区二区在线观看-国产中文字幕一区二区视频-精品一区二区三区av在线| 亚洲高清日本一区二区三区-日韩极品精品一区二区三区-亚洲成人av在线一区二区-亚洲精品国产精品粉嫩| 97资源视频在线观看-青草视频在线免费播放-最新日韩中文字幕在线播放-成人国产av精品麻豆网站| 国产美女口爆吞精服务-亚洲无人区码一码二码三码-久久精品99国产精品最新-日本少妇激情在线视频| 久久精品国产欧美日韩热-久久综合色一综合色88-特西西日本午夜人体艺术-97中文字幕在线视频| 少妇高潮了好爽在线观看男-麻豆国产传媒国产免费-欧美三级黄片在线播放-亚洲一区域二区域三区域四| 五月婷婷丁香综合入口-日本少妇免费中文字幕-96青草视频在线观看-中文字幕成人精品久久不卡| 亚洲黄色一级二级三级在线观看-成年人手机视频在线观看-都市激情校园春色亚洲一区-九九久久免费视频一区二区三区| 久久精品国产亚洲av麻豆看片-内射后入高潮在线视频-亚洲精品一区三区三区在线-亚洲乱码一区二区三区视色| 免费在线观看午夜视频-成人性生交大片免费网站-国产一区二区精品久久胖女人-亚州综合国产精品天码av| 日韩一区二区精品在线观看-日韩熟妇中文色在线视频-亚洲午夜精品免费福利-国产精品一区第二页尤自在拍| 国产精品剧情一区在线观看-精品伊人久久大香线蕉-一起草视频在线播放观看-精品少妇人妻av一区二区蜜桃| 91九色国产成人久久精品-亚洲av无一区二区三区av中文-最新日本加勒比在线视频-激情综合激情五月婷婷| 亚洲天堂av资源在线-四虎永久免费在线观看国产-久久这里只有精品人妻-欧美黄色三级经典精品| 日韩av手机在线观看免费-91精品人妻一区二区三区精-最近在线视频免费播放-国产亚洲欧洲在线观看| 办公室女厕偷拍美女撒尿-日本成人看片一区二区在线-丰满熟女少妇午夜福利-少妇被爽到高潮在线观看| 传媒精品视频在线观看-久久蜜汁成人国产精品-国产精品伦理视频一区三区-丰满少妇特黄一区二区三区| av网站在线观看网站-最新国产欧美精品91-国产一区二区三区在线导航-日韩高清在线中文字幕一区| 91精品18国产在线观看-午夜福利原创精品视频-欧美日韩在线亚洲另类-欧美日韩亚洲国产综合在线| 久久夜色国产精品亚洲-国产视频一区二区三区免费观看-亚洲一区二区成人在线观看-日韩精品一区二区三区在线视频| 国内一级一厂片内射视频播放磨-国产乐播传媒在线观看-让你操水蜜桃在线观看-深夜三级视频在线观看| 成人一区二区三区激情视频-久久一区二区免费蜜桃-钢琴考级三级咏叹调视频-亚洲性感毛片在线视频| 99久久亚洲综合精品成人网-国产性感丝袜在线观看-国产一区二区三区激情啪啪啪-久久香蕉综合国产蜜臀av| 久草免费福利在线播放-女同女同恋久久级三级-亚洲中文字母在线播放-91精品国产麻豆国产自产在| 日韩欧美国产亚洲中文-亚洲国产av第一福利网-亚洲欧洲日韩一区二区三区-91精品国产福利线观看久久|